ASTM C836-03
(Specification)Standard Specification for High Solids Content, Cold Liquid-Applied Elastomeric Waterproofing Membrane for Use with Separate Wearing Course
Standard Specification for High Solids Content, Cold Liquid-Applied Elastomeric Waterproofing Membrane for Use with Separate Wearing Course
SCOPE
1.1 This specification describes the required properties and test methods for a cold liquid-applied elastomeric-type membrane, one or two component, for waterproofing building decks subject to hydrostatic pressure in building areas to be occupied by personnel, vehicles, or equipment. This specification applies only to a membrane system above which a separate wearing or traffic course will be applied.
Note 1--See Guide C898 for proper application of membrane.
1.2 The values stated in SI units are to be regarded as the standard. The values given in parentheses are for information only.
1.3 The following safety hazards caveat pertains only to the test method portion, Section 6, of this specification. This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.
1.4 Ther are no ISO standards similar or equivalent to this ASTM standard.
General Information
Relations
Standards Content (Sample)
NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: C 836 – 03
Standard Specification for
High Solids Content, Cold Liquid-Applied Elastomeric
Waterproofing Membrane for Use with Separate Wearing
1
Course
This standard is issued under the fixed designation C 836; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (e) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the Department of Defense.
2
1. Scope Applied Waterproofing Membrane
C 1375 Guide for Substrates Used in Building Seals and
1.1 This specification describes the required properties and
2
Sealants
test methods for a cold liquid-applied elastomeric-type mem-
C 1471 Guide for the Use of High Solids Content Cold
brane,oneortwocomponent,forwaterproofingbuildingdecks
Liquid-Applied Elastomeric Waterproofing Membrane on
and walls subject to hydrostatic pressure in building areas to be
2
Vertical Surfaces
occupied by personnel, vehicles, or equipment. This specifica-
C 1522 Test Method for Extensibility After Heat Aging of
tionappliesonlytoamembranesystemabovewhichaseparate
2
Cold Liquid-Applied Waterproofing Membranes
wearing or traffic course will be applied.
D 2240 Test Method for Rubber Property—Durometer
NOTE 1—See Guide C 898 and Guide C 1471 for proper application of 3
Hardness
membrane.
2.2 Other Standards:
1.2 The values stated in SI units are to be regarded as the
CAM/CGSB-37.58 Membrane, Elastomeric, Cold-Applied
standard. The values given in parentheses are for information
Liquid, for Non-Exposed Use in Roofing and Waterproof-
4
only.
ing
1.3 This standard does not purport to address all of the
3. Terminology
safety concerns, if any, associated with its use. It is the
responsibility of the user of this standard to establish appro-
3.1 Definitions—RefertoTerminologyC 717fordefinitions
priate safety and health practices and determine the applica-
of the terms used in this standard.
bility of regulatory limitations prior to use.
4. Comparison to Other Standards
1.4 There are no ISO standards similar or equivalent to this
ASTM standard. 4.1 The committee with jurisdiction over this standard is
aware of one comparable standard published by another
2. Referenced Documents
organization. CAM/CGSB-37.58 has differences including a
2.1 ASTM Standards:
test method for Dimensional Stability and Water Absorption.
2
C 717 Terminology of Building Seals and Sealants
5. Physical Requirements
C 794 Test Method for Adhesion-in-Peel of Elastomeric
2
Joint Sealants
5.1 Material—Membrane materials shall cure, after appli-
C 898 Guide for Use of High Solids Content, Cold Liquid- cation by spreading or spraying, to form an elastomeric film
Applied Elastomeric Waterproofing Membrane with Sepa-
capable of maintaining a seal against liquid water.
2
rate Wearing Course 5.2 The physical, mechanical, and performance properties
C 1250 Test Method for Nonvolatile Content of Cold
of the membrane shall conform to the requirements described
2
Liquid-Applied Elastomeric Waterproofing Membranes in Table 1.
C 1305 Test Method for Crack Bridging Ability of Liquid-
6. Test Methods
6.1 Standard Conditions—Standard conditions for all tests
shall be 23 6 2°C (73.4 6 3.6°F) and 506 5 % relative
1
This specification is under the jurisdiction of ASTM Committee C24 on
humidity.
Building Seals and Sealants and is the direct responsibility of Subcommittee C24.80
on Building Deck Waterproofing Systems.
Current edition approved Feb. 10, 2003. Published April 2003. Originally
approved in 1976 as 836 – 76. Last previous edition approved in 2000 as
3
C 836 – 00. Annual Book of ASTM Standards, Vol 09.01.
2 4
Annual Book of ASTM Standards, Vol 04.07. Canadian General Standards Board, Ottawa, Canada, K1A 1G6.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.
1
---------------------- Page: 1 ----------------------
C836–03
TABLE 1 High Solids Content, Cold Liquid-Applied Elastomeric Waterproofing Membrane Physical Requirements
Property Requirement Test Method
Hardness, Type 00, min 50 D 2240 as modified in section 6.5 of
this specification
Weight loss, max, % 20 C 1250
Nonvolatile, min, % 80
Low temperature crack bridging no cracking C 1305
A
Film thickness (vertical surface), 1.5 6 0.1 (60 6 5) See section 6.8 of this specification
min, mm (mils)
Adhesion-in-Peel after water 175 (1) C 794 as modified in section 6.9 of
immersion, N/m (lbf/in.) this specification
Optional test for adhesion-in-peel No separation at See section 6.10 of this specification
interface
1
Extensibility after heat aging, min, 6.4 ( ⁄4), no cracking C 1522
mm (in.)
Stability, min, months 6 See section 6.12 of t
...







Questions, Comments and Discussion
Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.