Standard Specification for Copper-Cobalt-Beryllium and Copper-Nickel-Beryllium Rod and Bar (UNS Nos. C17500 and C17510)

SCOPE
1.1 This specification establishes the requirements for copper-cobalt-beryllium alloy (UNS No. C17500), and copper-nickel-beryllium alloy (UNS No. C17510) rod and bar in straight lengths.
1.2 The intent is to provide a system of interchangeable alloys.
1.3 Units—The values stated in inch-pound units are to be regarded as standard. The values given in parentheses are mathematical conversions to SI units, which are provided for information only and are not considered standard.
1.4 The following hazard statement pertains only to the test method portions of this specification: This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.

General Information

Status
Historical
Publication Date
09-Oct-2002
Current Stage
Ref Project

Relations

Buy Standard

Technical specification
ASTM B441-02 - Standard Specification for Copper-Cobalt-Beryllium and Copper-Nickel-Beryllium Rod and Bar (UNS Nos. C17500 and C17510)
English language
3 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: B 441 – 02
Standard Specification for
Copper-Cobalt-Beryllium and Copper-Nickel-Beryllium Rod
1
and Bar (UNS Nos. C17500 and C17510)
This standard is issued under the fixed designation B 441; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (e) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the Department of Defense.
1. Scope * E 1004 Practice for Determining Electrical Conductivity
5
Using the Electromagnetic (Eddy-Current) Method
1.1 This specification establishes the requirements for
copper-cobalt-beryllium alloy (UNS No. C17500), and copper-
3. General Requirements
nickel-beryllium alloy (UNS No. C17510) rod and bar in
3.1 The following sections of Specification B 249 constitute
straight lengths.
a part of this specification:
1.2 The intent is to provide a system of interchangeable
3.1.1 Terminology,
alloys.
3.1.2 Materials and Manufacture,
1.3 Units—The values stated in inch-pound units are to be
3.1.3 Dimensions and Permissible Variations,
regarded as standard. The values given in parentheses are
3.1.4 Workmanship, Finish, and Appearance,
mathematical conversions to SI units, which are provided for
3.1.5 Sampling,
information only and are not considered standard.
3.1.6 Number of Tests and Retests,
1.4 The following hazard statement pertains only to the test
3.1.7 Specimen Preparation,
method portions of this specification: This standard does not
3.1.8 Test Methods,
purport to address all of the safety concerns, if any, associated
3.1.9 Significance of Numerical Limits,
with its use. It is the responsibility of the user of this standard
3.1.10 Inspection,
to establish appropriate safety and health practices and
3.1.11 Rejection and Rehearing,
determine the applicability of regulatory limitations prior to
3.1.12 Certification,
use.
3.1.13 Test Report,
2. Referenced Documents 3.1.14 Packaging and Package Marking, and
3.1.15 Supplementary Requirements.
2.1 ASTM Standards:
3.2 In addition, when a section with a title identical to one
B 193 Test Method for Resistivity of Electrical Conductor
2
of those referenced in 3.1 appears in this specification, it
Materials
contains additional requirements that supplement those appear-
B 194 Specification for Copper-Beryllium Alloy Plate,
3
ing in Specification B 249.
Sheet, Strip and Rolled Bar
B 249 Specification for General Requirements for Wrought
4. Terminology
3
Copper and Copper-Alloy Rod, Bar, Shapes and Forgings
4.1 For definition of terms related to copper and copper
B 601 Classification for Temper Designations for Copper
3 alloys, refer to Terminology B 846.
and Copper Alloys—Wrought and Cast
3
B 846 Terminology for Copper and Copper Alloys
5. Ordering Information
4
E 8 Test Methods for Tension Testing of Metallic Materials
5.1 Include the following information in orders for product:
E 18 Test Methods for Rockwell Hardness and Rockwell
4 5.1.1 ASTM designation and year of issue,
Superficial Hardness of Metallic Materials
5.1.2 Copper alloy designation,
5.1.3 Temper (Section 7 and Table 1 and Table 2),
5.1.4 Form of product (cross section such as round, hexago-
1
This practice is under the jurisdiction of ASTM Committee B05 on Copper and
nal, octagonal, rectangular, or square),
Copper Alloys and is the direct responsibility of Subcommittee B05.02 on Rod, Bar,
5.1.5 Dimensions (diameter or distance between parallel
Wire, Shapes, and Forgings.
surfaces),
Current edition approved Oct. 10, 2002. Published November 2002. Originally
published as B 441 – 66. Last previous edition B 441 – 96.
2
Annual Book of ASTM Standards, Vol 02.03.
3
Annual Book of ASTM Standards, Vol 02.01.
4 5
Annual Book of ASTM Standards, Vol 03.01. Annual Book of ASTM Standards, Vol 03.03.
*A Summary of Changes section appears at the end of this standard.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.
1

---------------------- Page: 1 ----------------------
B441–02
A
TABLE 1 Tensile Strength and Rockwell Hardness Requirements for Rod and Bar
Temper Designation As Supplied
Tensile Electrical
Rockwell Hard-
Standard Former Strength, Conductivity
ness, B Scale
B C
ksi (MPa ) IACS min, %
TB00 solution heat-treated (A) 35–55 (240–380) 50 max 20
TD04 solution heat-treated and cold-worked: hard (H) 65–80 (450–550) 60–80 20
After Precipitation Heat Treatment
D
TF00 precipitation hardened (AT) 100–130 (690–895) 92–100 45
D
TH04 hard and precipitation heat-treated (HT) 110–140 (760–965) 95–102 48
A
These values apply to mill products. See Section 8 for exceptions in end products.
B
ksi = 1000 psi.
C
See Appendix.
D
Th
...