Standard Specification for Lap Cement Used with Asphalt Roll Roofing, Non-Fibered, and Fibered

ABSTRACT
This specification covers the physical requirements and testing of three types of lap cement for use with asphalt roll roofing. Type I is a brushing consistency lap cement intended for use in the exposed-nailing method of roll roofing application, and contains no mineral or other stabilizers. This type is further divided into two grades, as follows: Grade 1, which is made with an air-blown asphalt; and Grade 2, which is made with a vacuum-reduced or steam-refined asphalt. Both Types II and III, on the other hand, are heavy brushing or light troweling consistency lap cement intended for use in the concealed-nailing method of roll roofing application, only that Type II cement contains a quantity of short-fibered asbestos, while Type III cement contains a quantity of mineral or other stabilizers, or both, but contains no asbestos. The lap cements shall be sampled for testing, and shall adhere to specified values of the following properties: water content; distillation (total distillate at given temperatures); softening point of residue; solubility in trichloroethylene; and strength at indicated age.
SCOPE
1.1 This specification covers lap cement consisting of asphalt dissolved in a volatile petroleum solvent with or without mineral or other stabilizers, or both, for use with roll roofing. The fibered version of these cements excludes the use of asbestos fibers.  
1.2 The values stated in either SI units or inch-pound units are to be regarded separately as standard. The values stated in each system may not be exact equivalents; therefore, each system shall be used independently of the other. Combining values from the two systems may result in non-conformance with the standard.  
1.3 The following precautionary caveat applies only to the test method portion, Section 5, of this specification. This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.

General Information

Status
Historical
Publication Date
31-Dec-2016
Current Stage
Ref Project

Relations

Buy Standard

Technical specification
ASTM D3019/D3019M-17 - Standard Specification for Lap Cement Used with Asphalt Roll Roofing, Non-Fibered, and Fibered
English language
2 pages
sale 15% off
Preview
sale 15% off
Preview
Technical specification
REDLINE ASTM D3019/D3019M-17 - Standard Specification for Lap Cement Used with Asphalt Roll Roofing, Non-Fibered, and Fibered
English language
2 pages
sale 15% off
Preview
sale 15% off
Preview
Technical specification
ASTM D3019/D3019M-17 - Standard Specification for Lap Cement Used with Asphalt Roll Roofing, Non-Fibered, and Fibered
English language
2 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

This international standard was developed in accordance with internationally recognized principles on standardization established in the Decision on Principles for the
Development of International Standards, Guides and Recommendations issued by the World Trade Organization Technical Barriers to Trade (TBT) Committee.
Designation:D3019/D3019M −17
Standard Specification for
Lap Cement Used with Asphalt Roll Roofing, Non-Fibered,
1
and Fibered
This standard is issued under the fixed designation D3019/D3019M; the number immediately following the designation indicates the
year of original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last
reapproval. A superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope 3.1.1 Grade 1—Made with an air-blown asphalt.
3.1.2 Grade 2—Made with a vacuum-reduced or steam-
1.1 This specification covers lap cement consisting of as-
refined asphalt.
phalt dissolved in a volatile petroleum solvent with or without
mineral or other stabilizers, or both, for use with roll roofing. 3.2 Type III—Heavy brushing or light troweling consistency
The fibered version of these cements excludes the use of fibered lap cement intended for use in the concealed-nailing
asbestos fibers. methodofrollroofingapplication.TypeIIIlapcementcontains
a quantity of mineral or other stabilizers, or both, but contains
1.2 The values stated in either SI units or inch-pound units
no asbestos.
are to be regarded separately as standard. The values stated in
each system may not be exact equivalents; therefore, each
4. Physical Requirements
system shall be used independently of the other. Combining
4.1 The material shall conform to the requirements pre-
values from the two systems may result in non-conformance
scribed in Table 1.
with the standard.
1.3 The following precautionary caveat applies only to the
5. Sampling
test method portion, Section 5, of this specification. This
5.1 See Section 4, Sampling, of Test Methods D6511/
standard does not purport to address all of the safety concerns,
D6511M.
if any, associated with its use. It is the responsibility of the user
of this standard to establish appropriate safety and health
6. Test Methods
practices and determine the applicability of regulatory limita-
6.1 Determine composition and physical requirements by
tions prior to use.
using the procedures inTest Methods D6511/D6511M andTest
Method D36/D36M.
2. Referenced Documents
2
6.2 Strength of Lap:
2.1 ASTM Standards:
6.2.1 Significance—The lap strength is of importance only
D36/D36M Test Method for Softening Point of Bitumen
for Type III cement used in the concealed-nailing method of
(Ring-and-Ball Apparatus)
roll roofing application.
D6511/D6511M Test Methods for Solvent Bearing Bitumi-
nous Compounds
7. Inspection
3. Classification 7.1 Inspection of the material shall be as agreed upon
between the purchaser and the supplier as part of the purchase
3.1 Type I—Brushing consistency non-fibered lap cement
contract.
intended for use in the exposed-nailing method of roll roofing
application. Type I lap cement contains no mineral or other
8. Rejection and Resubmittal
stabilizers.
8.1 Failure to conform to any of the requirements prescribed
in this specification may constitute grounds for rejection. In the
1
This specification is under the jurisdiction of ASTM Committee D08 on
case of rejection, the seller shall h
...

This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
Designation: D3019 − 08 D3019/D3019M − 17
Standard Specification for
Lap Cement Used with Asphalt Roll Roofing, Non-Fibered,
1
Asbestos-Fibered, and Non-Asbestos-FiberedFibered
This standard is issued under the fixed designation D3019;D3019/D3019M; the number immediately following the designation indicates
the year of original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last
reapproval. A superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope
1.1 This specification covers lap cement consisting of asphalt dissolved in a volatile petroleum solvent with or without mineral
or other stabilizers, or both, for use with roll roofing. The fibered version of these cements excludes the use of asbestos fibers.
1.2 The values stated in either SI units or inch-pound units are to be regarded separately as the standard. The values given in
parentheses are for information only. stated in each system may not be exact equivalents; therefore, each system shall be used
independently of the other. Combining values from the two systems may result in non-conformance with the standard.
1.3 The following precautionary caveat applies only to the test method portion, Section 5, of this specification. This standard
does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this
standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.
2. Referenced Documents
2
2.1 ASTM Standards:
D36D36/D36M Test Method for Softening Point of Bitumen (Ring-and-Ball Apparatus)
D6511D6511/D6511M Test Methods for Solvent Bearing Bituminous Compounds
3. Classification
3.1 Type I—Brushing consistency non-fibered lap cement intended for use in the exposed-nailing method of roll roofing
application. Type I lap cement contains no mineral or other stabilizers.
3.1.1 Grade 1—Made with an air-blown asphalt.
3.1.2 Grade 2—Made with a vacuum-reduced or steam-refined asphalt.
3.2 Type II—Heavy brushing or light troweling consistency lap cement intended for use in the concealed-nailing method of roll
roofing application. Type II lap cement contains a quantity of short-fibered asbestos.
3.2 Type III—Heavy brushing or light troweling consistency fibered lap cement intended for use in the concealed-nailing method
of roll roofing application. Type III lap cement contains a quantity of mineral or other stabilizers, or both, but contains no asbestos.
4. Physical Requirements
4.1 The material shall conform to the requirements prescribed in Table 1.
5. Sampling
5.1 See Section 4, Sampling, of Test Methods D6511D6511/D6511M.
6. Test Methods
6.1 Determine composition and physical requirements by using the procedures in Test Methods D6511D6511/D6511M and Test
Method D36D36/D36M.
6.2 Strength of Lap:
1
This specification is under the jurisdiction of ASTM Committee D08 on Roofing and Waterproofing and is the direct responsibility of Subcommittee D08.05 on
Solvent-Bearing Bituminous Compounds for Roofing and Waterproofing.
Current edition approved Feb. 15, 2008Jan. 1, 2017. Published March 2008January 2017. Originally approved in 1972. Last previous edition approved in 20072008 as
D3019 – 94 (2007).D3019 – 08. DOI: 10.1520/D3019-08.10.1520/D3019_D3019M-17.
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards
volume information, refer to the standard’s Document Summary page on the ASTM website.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
D3019/D3019M − 17
TABLE 1 Requirements for Lap Cement
Type I
Grade 1 Grade 2 Type IIIII Type III
min max min max
Water, volume percent of original sample . 0.5 . 0.5 0.5 max 2.5 max
Water, volume percent of original sample . 0.5 . 0.5 2.5 max
Distillation, total distillate to each temperature,
volume percent of original sample:
to 190°C (374°F) 5 20 2 20 . .
to 190°C [374°F] 5 20 2 20 .
to 225°C (437°F) 15 35 15 35 . .
to 225°C [437°F] 15 35 15 35 .
to 260°C (500°F) 25 40 25 40 . .
to 260°C [500°F] 25 40 25 40 .
to 316°C (600°F) 30 45 30 45 . .
to 316°C [600°F] 30 45 30 45 .
to 360°C (680°F) . 50 . 50 . .
to 360°C [680°F] . 50 . 50 .
Softening point of residue from distillation, °C (° F) 57 (135) . 41
...

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D3019/D3019M − 17
Standard Specification for
Lap Cement Used with Asphalt Roll Roofing, Non-Fibered,
1
and Fibered
This standard is issued under the fixed designation D3019/D3019M; the number immediately following the designation indicates the
year of original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last
reapproval. A superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope 3.1.1 Grade 1—Made with an air-blown asphalt.
3.1.2 Grade 2—Made with a vacuum-reduced or steam-
1.1 This specification covers lap cement consisting of as-
refined asphalt.
phalt dissolved in a volatile petroleum solvent with or without
mineral or other stabilizers, or both, for use with roll roofing. 3.2 Type III—Heavy brushing or light troweling consistency
The fibered version of these cements excludes the use of fibered lap cement intended for use in the concealed-nailing
asbestos fibers. method of roll roofing application. Type III lap cement contains
a quantity of mineral or other stabilizers, or both, but contains
1.2 The values stated in either SI units or inch-pound units
no asbestos.
are to be regarded separately as standard. The values stated in
each system may not be exact equivalents; therefore, each
4. Physical Requirements
system shall be used independently of the other. Combining
4.1 The material shall conform to the requirements pre-
values from the two systems may result in non-conformance
scribed in Table 1.
with the standard.
1.3 The following precautionary caveat applies only to the
5. Sampling
test method portion, Section 5, of this specification. This
5.1 See Section 4, Sampling, of Test Methods D6511/
standard does not purport to address all of the safety concerns,
D6511M.
if any, associated with its use. It is the responsibility of the user
of this standard to establish appropriate safety and health
6. Test Methods
practices and determine the applicability of regulatory limita-
6.1 Determine composition and physical requirements by
tions prior to use.
using the procedures in Test Methods D6511/D6511M and Test
Method D36/D36M.
2. Referenced Documents
2
6.2 Strength of Lap:
2.1 ASTM Standards:
6.2.1 Significance—The lap strength is of importance only
D36/D36M Test Method for Softening Point of Bitumen
for Type III cement used in the concealed-nailing method of
(Ring-and-Ball Apparatus)
roll roofing application.
D6511/D6511M Test Methods for Solvent Bearing Bitumi-
nous Compounds
7. Inspection
3. Classification 7.1 Inspection of the material shall be as agreed upon
between the purchaser and the supplier as part of the purchase
3.1 Type I—Brushing consistency non-fibered lap cement
contract.
intended for use in the exposed-nailing method of roll roofing
application. Type I lap cement contains no mineral or other
8. Rejection and Resubmittal
stabilizers.
8.1 Failure to conform to any of the requirements prescribed
in this specification may constitute grounds for rejection. In the
1
This specification is under the jurisdiction of ASTM Committee D08 on case of rejection, the seller shall have the right to reinspect the
Roofing and Waterproofing and is the direct resp
...

Questions, Comments and Discussion

Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.