Standard Test Method for Hexane/Petroleum Ether Extract in Wet Blue and Wet White

SIGNIFICANCE AND USE
4.1 This test method measures the amount of solvent-soluble (hexane or petroleum ether) materials in wet blue and wet white.
SCOPE
1.1 This test method covers the quantitative extraction of all types of wet blue and wet white with hexane or petroleum ether.  
1.2 The values stated in SI units are to be regarded as the standard. The values given in parentheses are for information only.  
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use. For a specific hazard statement, see Section 7.

General Information

Status
Historical
Publication Date
31-Mar-2014
Technical Committee
Drafting Committee
Current Stage
Ref Project

Relations

Buy Standard

Standard
ASTM D7674-14 - Standard Test Method for Hexane/Petroleum Ether Extract in Wet Blue and Wet White
English language
4 pages
sale 15% off
Preview
sale 15% off
Preview
Standard
REDLINE ASTM D7674-14 - Standard Test Method for Hexane/Petroleum Ether Extract in Wet Blue and Wet White
English language
4 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D7674 − 14
StandardTest Method for
1
Hexane/Petroleum Ether Extract in Wet Blue and Wet White
This standard is issued under the fixed designation D7674; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope 4. Significance and Use
1.1 This test method covers the quantitative extraction of all 4.1 This test method measures the amount of solvent-
types of wet blue and wet white with hexane or petroleum soluble (hexane or petroleum ether) materials in wet blue and
ether. wet white.
1.2 The values stated in SI units are to be regarded as the
5. Apparatus
standard. The values given in parentheses are for information
5.1 Analytical Balance.
only.
5.2 Extraction Apparatus—Soxhlet, consisting of a boiling
1.3 This standard does not purport to address all of the
flask, extraction tube, and condenser. Alternate Extraction
safety concerns, if any, associated with its use. It is the
Apparatus: Soxtec-type system consisting of an extraction unit
responsibility of the user of this standard to establish appro-
and a control unit.
priate safety and health practices and determine the applica-
bility of regulatory limitations prior to use. For a specific
5.3 ForcedCirculatingAirOven,capableofmaintainingthe
hazard statement, see Section 7.
specified temperature.
5.4 Electric Hot Plate (or steam bath).
2. Referenced Documents
2
5.5 Extraction Thimbles, fat-free: cellulose,Alundum, glass
2.1 ASTM Standards:
microfiber, or fritted glass.
D3495 Test Method for Hexane Extraction of Leather
D6658 Test Method for Volatile Matter (Moisture) of Wet 5.6 Absorbent Cotton, fat-free, or glass wool.
Blue by Oven Drying
6. Reagents and Materials
D6659 Practice for Sampling and Preparation of Wet Blue
for Physical and Chemical Tests
6.1 Hexane, ACS Reagent Grade, or
E691 Practice for Conducting an Interlaboratory Study to
6.2 Petroleum Ether, ACS Reagent Grade.
Determine the Precision of a Test Method
E177 Practice for Use of the Terms Precision and Bias in
7. Hazards
ASTM Test Methods
7.1 All reagents and chemicals should be handled with care.
Before using any chemical, read and follow all safety precau-
3. Summary of Test Method
tions and instructions on the manufacturers’ label or MSDS
3.1 A specimen is analyzed as received in wet state, diced;
(Material Safety Data Sheet).
or pre-dried at the determined setting then ground prior to
analysis. The prepared specimen is extracted with solvent. 8. Sampling
Another specimen from the same sample is also analyzed for
8.1 The wet blue or wet white shall be sampled in accor-
moisture content in accordance with Test Method D6658.
dance with Test Method D6659.
Following completion of the extraction process, the extract is
dried, then cooled and weighed. The extract is reported as
9. Procedure
extractables on a moisture-free basis. NOTE 1—Two sample conditions are listed below. Both sample condi-
tions produce acceptable results (See Precision and Bias section).
9.1 Condition A—As received in wet state, diced (prepared
1
This test method is under the jurisdiction ofASTM Committee D31 on Leather
per Test Method D6659 Method A).
and is the direct responsibility of Subcommittee D31.02 on Wet Blue.
9.1.1 Weigh out specimen for both moisture and hexane/
Current edition approved April 1, 2014. Published June 2014. DOI: 10.1520/
D7674-14.
petroleum ether extraction at the same time. For the hexane/
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or
petroleum ether extraction, weigh an 8-10 g specimen to the
contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM
nearest 0.001g and record this value as W1. Loosely pack the
Standards volume information, refer to the standard’s Document Summary page on
the ASTM website. material in an appropriately sized extraction thimble and cover
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
D7674 − 14
with a pad of fat-free cotton or glass wool. Proceed with circulating oven at 100 6 2°C (212 6 3.6°F) for 60-65 min or
extractionusingeithertheSoxhletapparatusortheSoxtec-type 25-30 min at 125 6 1°C (257 6 1.8°F). Cool the cups for
apparatus. 30-35 min (or to room temperature) in a desiccator. Continue
9.1.2 Determine the moisture content of the prepared drying for successive 15-min periods until constant weight is
sample from which the specimen for extraction is taken (9.1.1) obtained. When successive weighings vary by less than
in accordance with Test Method D6658. 60.005 g, consider t
...

This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
Designation: D7674 − 10 D7674 − 14
Standard Test Method for
1
Hexane/Petroleum Ether Extract in Wet Blue and Wet White
This standard is issued under the fixed designation D7674; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope
1.1 This test method covers the quantitative extraction of all types of wet blue and wet white with hexane or petroleum ether.
1.2 The values stated in SI units are to be regarded as the standard. The values given in parentheses are for information only.
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility
of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory
limitations prior to use. For a specific hazard statement, see Section 7.
2. Referenced Documents
2
2.1 ASTM Standards:
D3495 Test Method for Hexane Extraction of Leather
D6658 Test Method for Volatile Matter (Moisture) of Wet Blue by Oven Drying
D6659 Practice for Sampling and Preparation of Wet Blue for Physical and Chemical Tests
E691 Practice for Conducting an Interlaboratory Study to Determine the Precision of a Test Method
E177 Practice for Use of the Terms Precision and Bias in ASTM Test Methods
3. Summary of Test Method
3.1 A specimen is analyzed as received in wet state, diced; or pre-dried at the determined setting then ground prior to analysis.
The prepared specimen is extracted with solvent. Another specimen from the same sample is also analyzed for moisture content
in accordance with Test Method D6658. Following completion of the extraction process, the extract is dried, then cooled and
weighed. The extract is reported as extractables on a moisture-free basis.
4. Significance and Use
4.1 This test method measures the amount of solvent-soluble (hexane or petroleum ether) materials in wet blue and wet white.
5. Apparatus
5.1 Analytical Balance.
5.2 Extraction Apparatus—Soxhlet, consisting of a boiling flask, extraction tube, and condenser. Alternate Extraction
Apparatus: Soxtec-type system consisting of an extraction unit and a control unit.
5.3 Forced Circulating Air Oven, capable of maintaining the specified temperature.
5.4 Electric Hot Plate (or steam bath).
5.5 Extraction Thimbles, fat-free: cellulose, Alundum, glass microfiber, or fritted glass.
5.6 Absorbent Cotton, fat-free, or glass wool.
6. Reagents and Materials
6.1 Hexane, ACS Reagent Grade, or
6.2 Petroleum Ether, ACS Reagent Grade.
1
This test method is under the jurisdiction of ASTM Committee D31 on Leather and is the direct responsibility of Subcommittee D31.02 on Wet Blue.
Current edition approved Nov. 1, 2010April 1, 2014. Published December 2010June 2014. DOI: 10.1520/D7674-10.10.1520/D7674-14.
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards
volume information, refer to the standard’s Document Summary page on the ASTM website.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
D7674 − 14
7. Hazards
7.1 All reagents and chemicals should be handled with care. Before using any chemical, read and follow all safety precautions
and instructions on the manufacturers’ label or MSDS (Material Safety Data Sheet).
8. Sampling
8.1 The wet blue or wet white shall be sampled in accordance with Test Method D6659.
9. Procedure
NOTE 1—Two sample conditions are listed below. Both sample conditions produce acceptable results (See Precision and Bias section).
9.1 Condition A—As received in wet state, diced (prepared per Test Method D6659 Method A).
9.1.1 Weigh out specimen for both moisture and hexane/petroleum ether extraction at the same time. For the hexane/petroleum
ether extraction, weigh an 8-10 g specimen to the nearest 0.001g and record this value as W1. Loosely pack the material in an
appropriately sized extraction thimble and cover with a pad of fat-free cotton or glass wool. Proceed with extraction using either
the Soxhlet apparatus or the Soxtec-type apparatus.
9.1.2 Determine the moisture content of the prepared sample from which the specimen for extraction is taken (9.1.1) in
accordance wi
...

Questions, Comments and Discussion

Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.