ASTM D2200-17
(Practice)Standard Practice for Use of Pictorial Surface Preparation Standards and Guides for Painting Steel Surfaces
Standard Practice for Use of Pictorial Surface Preparation Standards and Guides for Painting Steel Surfaces
SIGNIFICANCE AND USE
4.1 The appearance of the various degrees of dry and wet abrasive blast cleaning, hand and power tool cleaning and water jetting are influenced by the initial rust grades of the steel being cleaned and/or the type and condition of the coating on the existing steel. The standards and guides aid visually in judging and evaluating the degree of rusting and/or paint deterioration before cleaning and the degree of cleaning of steel surfaces prior to painting.
4.2 Five methods have evolved because of differences in the practice of using visual standards and guides throughout the world, and the method of surface preparation employed. In Europe, the visual standards (Method A) are used as the primary means of assessing the degree of cleaning. In the US, the SSPC written definitions take precedence with the visual guides and reference photographs used as a supplement. The visual guides and reference photographs of Methods B, C, and D conform to the SSPC written definitions. There are written definitions for Method E, however, the visual guide for Method E does not contain a complete set of pictorials corresponding to each surface cleanliness definition.
SCOPE
1.1 The visual surface preparation guides and standards consist of a series of color prints available as separate publications. Five different sets of photographs are described in this standard, designated as Method A (ISO/Swedish Standard2) and Methods B through E (SSPC Guides and Reference Photographs3). The methods differ in the depiction of the initial surface, in the definition and depiction of the cleaning conditions, and in the number of cleaning methods included. Because of these differences, the specifier should state which guide to use.
1.2 The colored visual surface preparation guides represent different conditions of hot rolled carbon steel before and after surface preparation. Prior to cleaning, there are four rust grades, A to D, that cover the range from intact mill scale to 100 % rusted and pitted steel. The standards then depict the appearance of the initial conditions after cleaning by one or more methods (for example, dry abrasive blast cleaning) to various degrees of thoroughness. In addition, Method B includes three painted conditions that contain various degrees of deterioration. The Guide3 depicts these conditions after various degrees of dry abrasive blast cleaning. Method C includes four rust grades and three painted conditions that contain various degrees of deterioration. The Guide4 depicts these conditions after various degrees of hand and power tool cleaning. Method D includes two rust grades and four painted conditions that contain various degrees of deterioration. The Guide5 depicts these conditions after various degrees of water jetting, with three levels of flash rusting. Method E includes two rust grades. The Guide6 depicts these conditions after various degrees of wet abrasive blast cleaning, with three levels of flash rusting.
1.3 This international standard was developed in accordance with internationally recognized principles on standardization established in the Decision on Principles for the Development of International Standards, Guides and Recommendations issued by the World Trade Organization Technical Barriers to Trade (TBT) Committee.
General Information
Buy Standard
Standards Content (Sample)
NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D2200 − 17 Swedish Standards Association
Standard SIS 05 59 00
ISO 8501
SSPC: The Society for Protective Coatings
SSPC VIS 1, VIS 3, VIS 4/NACE VIS 7, VIS 5/NACE VIS 9
Danish Standards Association
Danish Standard DS 2019
European Committee of Paint and Printing
Ink Manufacturers’Association
Standard Practice for
Use of Pictorial Surface Preparation Standards and Guides
1
for Painting Steel Surfaces
This standard is issued under the fixed designation D2200; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the U.S. Department of Defense.
1. Scope various degrees of dry abrasive blast cleaning. Method C
includes four rust grades and three painted conditions that
1.1 The visual surface preparation guides and standards
4
contain various degrees of deterioration. The Guide depicts
consist of a series of color prints available as separate
these conditions after various degrees of hand and power tool
publications.Fivedifferentsetsofphotographsaredescribedin
cleaning. Method D includes two rust grades and four painted
this standard, designated as Method A (ISO/Swedish Stan-
2 conditions that contain various degrees of deterioration. The
dard ) and Methods B through E (SSPC Guides and Reference
5
3
Guide depicts these conditions after various degrees of water
Photographs ).Themethodsdifferinthedepictionoftheinitial
jetting, with three levels of flash rusting. Method E includes
surface, in the definition and depiction of the cleaning
6
two rust grades. The Guide depicts these conditions after
conditions, and in the number of cleaning methods included.
various degrees of wet abrasive blast cleaning, with three
Because of these differences, the specifier should state which
levels of flash rusting.
guide to use.
1.3 This international standard was developed in accor-
1.2 The colored visual surface preparation guides represent
dance with internationally recognized principles on standard-
different conditions of hot rolled carbon steel before and after
ization established in the Decision on Principles for the
surface preparation. Prior to cleaning, there are four rust
Development of International Standards, Guides and Recom-
grades, A to D, that cover the range from intact mill scale to
mendations issued by the World Trade Organization Technical
100 % rusted and pitted steel. The standards then depict the
Barriers to Trade (TBT) Committee.
appearance of the initial conditions after cleaning by one or
more methods (for example, dry abrasive blast cleaning) to
2. Referenced Documents
various degrees of thoroughness. In addition, Method B
2.1 Other Documents:
includes three painted conditions that contain various degrees
2,3,4,5,6
3 Pictorial Surface Preparation Standards and Guides
of deterioration. The Guide depicts these conditions after
3,4
Surface Cleanliness Definitions
3. Terminology
1
This practice is under the jurisdiction of ASTM Committee D01 on Paint and
Related Coatings, Materials, and Applications and is the direct responsibility of
3.1 Definitions:
Subcommittee D01.46 on Industrial Protective Coatings.
3.1.1 The cleanliness definitions for the Method A visual
The pictorial standards described were prepared by the Swedish Corrosion
surface preparation standard appear in the text of the pictorial
Institute and have been jointly approved by ASTM, The Society For Protective
Coatings (SSPC) (VIS 1), and the Swedish Standardizing Commission.
Current edition approved Dec. 1, 2017. Published December 2017. Originally
4
approved in 1966. Last previous edition approved in 2013 as D2200 – 13. DOI: The Visual Guide for Method C and the surface cleanliness definitions are
10.1520/D2200-17. available from The Society for Protective Coatings (SSPC), 800 Trumbull Drive,
2
The pictorial surface preparation standard Method A is available from The Pittsburgh, PA 15205-4365, http://www.sspc.org.
5
Society for Protective Coatings (SSPC), 800 Trumbull Drive, Pittsburgh, PA The Visual Guide for Method D and the surface cleanliness definitions are
15205-4365, http://www.sspc.org and Sveriges Standardiseringskommission, Box available from The Society for Protective Coatings (SSPC), 800 Trumbull Drive,
3295, Stockholm 3, Sweden. Pittsburgh, PA 15205-4365, http://www.sspc.org.
3 6
TheVisualGuideforMethodBandsurfacecleanlinessdefinitionsareavailable The Visual Guide for Method E and the surface cleanliness definitions are
from The Society for Protective Coatings (SSPC), 800 Trumbull Drive, Pittsburgh, available from The Society for Protective Coatings (SSPC), 800 Trumbull Dr
...
This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
Designation: D2200 − 13 D2200 − 17 Swedish Standards Association
Standard SIS 05 59 00
ISO 8501
SSPC: The Society for Protective Coatings
SSPC VIS 1, VIS 3, VIS 4/NACE VIS 7, VIS 5/NACE VIS 9
Danish Standards Association
Danish Standard DS 2019
European Committee of Paint and Printing
Ink Manufacturers’Manufacturers’ Association
Standard Practice for
Use of Pictorial Surface Preparation Standards and Guides
1
for Painting Steel Surfaces
This standard is issued under the fixed designation D2200; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the U.S. Department of Defense.
1. Scope
1.1 The visual surface preparation guides and standards consist of a series of color prints available as separate publications. Five
2
different sets of photographs are described in this standard, designated as Method A (ISO/Swedish Standard ) and Methods B
3
through E (SSPC Guides and Reference Photographs ). The methods differ in the depiction of the initial surface, in the definition
and depiction of the cleaning conditions, and in the number of cleaning methods included. Because of these differences, the
specifier should state which methodguide to use.
1.2 The colored visual surface preparation guides represent different conditions of hot rolled carbon steel before and after
surface preparation. Prior to cleaning, there are four rust grades, A to D, that cover the range from intact mill scale to 100 % rusted
and pitted steel. The standards then depict the appearance of the initial conditions after cleaning by one or more methods (for
example, dry abrasive blast cleaning) to various degrees of thoroughness. In addition, Method B includes three painted conditions
3
that contain various degrees of deterioration. The Guide depicts these conditions after various degrees of dry abrasive blast
4
cleaning. Method C includes four rust grades and three painted conditions that contain various degrees of deterioration. The Guide
depicts these conditions after various degrees of hand and power tool cleaning. Method D includes two rust grades and four painted
5
conditions that contain various degrees of deterioration. The Guide depicts these conditions after various degrees of water jetting,
6
with three levels of flash rusting. Method E includes two rust grades. The Guide depicts these conditions after various degrees
of wet abrasive blast cleaning, with three levels of flash rusting.
1.3 This international standard was developed in accordance with internationally recognized principles on standardization
established in the Decision on Principles for the Development of International Standards, Guides and Recommendations issued
by the World Trade Organization Technical Barriers to Trade (TBT) Committee.
1
This practice is under the jurisdiction of ASTM Committee D01 on Paint and Related Coatings, Materials, and Applications and is the direct responsibility of
Subcommittee D01.46 on Industrial Protective Coatings.
The pictorial standards described were prepared by the Swedish Corrosion Institute and have been jointly approved by ASTM, The Society For Protective Coatings (SSPC)
(VIS 1), and the Swedish Standardizing Commission.
Current edition approved June 1, 2013Dec. 1, 2017. Published July 2013December 2017. Originally approved in 1966. Last previous edition approved in 20082013 as
D2200 – 08.D2200 – 13. DOI: 10.1520/D2200-13.10.1520/D2200-17.
2
The pictorial surface preparation standard Method A is available from The Society for Protective Coatings (SSPC), 40 24th St., 6th Floor, 800 Trumbull Drive, Pittsburgh,
PA 15222-4656,15205-4365, http://www.sspc.org and Sveriges Standardiseringskommission, Box 3295, Stockholm 3, Sweden.
3
The Visual Guide for Method B and surface cleanliness definitions are available from The Society for Protective Coatings (SSPC), 40 24th St., 6th Floor, 800 Trumbull
Drive, Pittsburgh, PA 15222-4656,15205-4365, http://www.sspc.org.
4
The Visual Guide for Method C and the surface cleanliness definitions are available from The Society for Protective Coatings (SSPC), 40 24th St., 6th Floor, 800 Trumbull
Drive, Pittsburgh, PA 15222-4656,15205-4365, http://www.sspc.org.
5
The Visual Guide for Method D and the surface cleanliness definitions are available from The Society for Protective Coa
...
Questions, Comments and Discussion
Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.