ASTM D3591-97(2003)
(Test Method)Standard Test Method for Determining Logarithmic Viscosity Number of Poly(Vinyl Chloride) (PVC) in Formulated Compounds
Standard Test Method for Determining Logarithmic Viscosity Number of Poly(Vinyl Chloride) (PVC) in Formulated Compounds
SIGNIFICANCE AND USE
The logarithmic viscosity number provides information on the effect of compounding or processing of PVC.
Exposure of PVC compositions to shear or to high temperatures can result in a change in the logarithmic viscosity number of the resin.
SCOPE
1.1 This test method covers the determination of the logarithmic viscosity number of poly(vinyl chloride) (PVC) homopolymers after compounding or processing.
1.2 It is the basic assumption of this technique that the formulation of the compounded resin is known and that any additives present can be separated from the resin by extraction with diethyl ether. This is necessary to permit adjustment of the amount of sample used in the test to give a resin concentration in cyclohexanone of 0.2 ± 0.002 g/100 mL.
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use. Specific precautionary statements are given in 7.3 and 8.4.1.
General Information
Relations
Standards Content (Sample)
NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation:D3591–97 (Reapproved 2003)
Standard Test Method for
Determining Logarithmic Viscosity Number of Poly(Vinyl
1
Chloride) (PVC) in Formulated Compounds
This standard is issued under the fixed designation D3591; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope* System of Units (SI)
2.2 ISO Standard:
1.1 This test method covers the determination of the loga-
1628-2 Plastics—Determination of Viscosity Number and
rithmic viscosity number of poly(vinyl chloride) (PVC) ho-
Limiting Viscosity Number—Part 2: Poly (Vinyl Chlo-
mopolymers after compounding or processing.
3
ride) Resins
1.2 It is the basic assumption of this technique that the
formulation of the compounded resin is known and that any
3. Terminology
additives present can be separated from the resin by extraction
3.1 Units and symbols used in this test method are those
withdiethylether.Thisisnecessarytopermitadjustmentofthe
recommended in IEEE/ASTM SI-10.
amount of sample used in the test to give a resin concentration
3.2 Definitions of Terms Specific to This Standard:
in cyclohexanone of 0.2 6 0.002 g/100 mL.
3.2.1 The term logarithmic viscosity number is defined by
1.3 This standard does not purport to address all of the
the equation is 9.1.
safety concerns, if any, associated with its use. It is the
responsibility of the user of this standard to establish appro-
4. Summary of Test Method
priate safety and health practices and determine the applica-
4.1 The sample is pressed into a thin film and extracted to
bility of regulatory limitations prior to use. Specific precau-
remove the plasticizer.
tionary statements are given in 7.3 and 8.4.1.
4.2 The plasticizer-free film is dissolved in cyclohexanone
NOTE 1—This test method and ISO 1628-2 are not equivalent.
and centrifuged to remove insoluble matter.
4.3 Theviscosityofthecyclohexanonesolutionismeasured
2. Referenced Documents
in accordance with Test Method D1243.
2
2.1 ASTM Standards:
D445 Test Method for Kinematic Viscosity of Transparent 5. Significance and Use
and Opaque Liquids (and Calculation of Dynamic Viscos-
5.1 The logarithmic viscosity number provides information
ity)
on the effect of compounding or processing of PVC.
D446 Specifications and Operating Instructions for Glass
5.2 Exposure of PVC compositions to shear or to high
Capillary Kinematic Viscometers
temperatures can result in a change in the logarithmic viscosity
D1243 Test Method for Dilute Solution Viscosity of Vinyl
number of the resin.
Chloride Polymers
6. Apparatus
D2124 Test Method for Analysis of Components in Poly-
(Vinyl Chloride) Compounds Using an Infrared Spectro-
6.1 Centrifuge, capable of 2500 rpm with 100-mL sample
photometric Technique
container.
E1 Specification for ASTM Liquid-in-Glass Thermometers
6.2 Heated Hydraulic Press, capable of 620-kN ram force
E691 Practice for Conducting an Interlaboratory Study to
and a temperature of 165°C.
Determine the Precision of a Test Method
6.3 Soxhlet Extraction Apparatus with a 150-mL flask and
IEEE/ASTM SI-10 Standard for the Use of International
a 27 by 100-mm thimble.
6.4 Volumetric Flasks, 100-mL.
4
6.5 Viscometers.
1
This test method is under the jurisdiction ofASTM Committee D20 on Plastics
6.6 Infrared Spectrophotometer, see 5.4 of Method D2124.
and is the direct responsibility of Subcommittee D20.70 on Analytical Methods.
Current edition approved March 10, 2003. Published April 2003. Originally
approved in 1977. Last previous edition approved in 1997 as D3591 – 97. DOI:
10.1520/D3591-97R03.
2 3
For referenced ASTM standards, visit the ASTM website, www.astm.org, or Available fromAmerican National Standards Institute (ANSI), 25 W. 43rd St.,
contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM 4th Floor, New York, NY 10036, http://www.ansi.org.
4
Standards volume information, refer to the standard’s Document Summary page on Cannon Fenske No. 75 or Ubbelohde No. 1 have been found satisfactory for
the ASTM website. this purpose.
*A Summary of Changes section appears at the end of this standard.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.
1
---------------------- Page: 1 ----------------------
D3591–97 (2003)
7. Reagents
7.1 Cyclohexanone, high-purity (see Annex A1).
7.2 Diethyl Ether, anhydrous, reagent grade.
7.3 (Warning—Safety precautions should be taken to avoid
personal contact, to eliminate toxic vapors, and to guard
against explosive hazards in accordance with the hazardous
nature of the particular reagent being used.)
8. Procedure
8.1 Prepare the PVC s
...
Questions, Comments and Discussion