Standard Test Method for Measuring Thickness of Leather Test Specimens

SIGNIFICANCE AND USE
3.1 This test method shall be used where precise dimensions are necessary for calculation of properties expressed in physical units. It is not intended to replace practical thickness measurements based on commercial portable tools, nor is it implied that thickness measurements made by the two procedures will agree exactly.
SCOPE
1.1 This test method covers the measurement of the thickness of leather test specimens in which the dimensions of the specimens are used directly in determining the results of tests for physical properties. This test method does not apply to wet blue.  
1.2 The values stated in inch-pound units are to be regarded as standard. The values given in parentheses are mathematical conversions to SI units that are provided for information only and are not considered standard.  
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety, health, and environmental practices and determine the applicability of regulatory limitations prior to use.  
1.4 This international standard was developed in accordance with internationally recognized principles on standardization established in the Decision on Principles for the Development of International Standards, Guides and Recommendations issued by the World Trade Organization Technical Barriers to Trade (TBT) Committee.

General Information

Status
Historical
Publication Date
31-Aug-2017
Technical Committee
Drafting Committee
Current Stage
Ref Project

Buy Standard

Standard
ASTM D1813-13(2017) - Standard Test Method for Measuring Thickness of Leather Test Specimens
English language
2 pages
sale 15% off
Preview
sale 15% off
Preview
Standard
REDLINE ASTM D1813-13(2017) - Standard Test Method for Measuring Thickness of Leather Test Specimens
English language
2 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D1813 − 13 (Reapproved 2017)
Standard Test Method for
1
Measuring Thickness of Leather Test Specimens
This standard is issued under the fixed designation D1813; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the U.S. Department of Defense.
1. Scope measurements based on commercial portable tools, nor is it
implied that thickness measurements made by the two proce-
1.1 This test method covers the measurement of the thick-
dures will agree exactly.
ness of leather test specimens in which the dimensions of the
specimens are used directly in determining the results of tests
4. Apparatus
for physical properties. This test method does not apply to wet
4.1 Gage, equipped with a dial micrometer, a flat anvil, and
blue.
3
a presser foot loaded by a dead mass.
1.2 The values stated in inch-pound units are to be regarded
4.2 Dial, graduated to read to the nearest 0.01 mm, with
as standard. The values given in parentheses are mathematical
small second dial graduated to read to the nearest 1 mm or to
conversions to SI units that are provided for information only
the nearest 0.001 in. and 0.1 in. respectively.
and are not considered standard.
1.3 This standard does not purport to address all of the 4.3 Anvil, flat, with a diameter of 0.395 6 0.02 in. (10 6 0.5
safety concerns, if any, associated with its use. It is the mm) and projecting 0.1 in. (2.5 mm) from the surface of a flat
circular platform about 2 in. (50 mm) in diameter.
responsibility of the user of this standard to establish appro-
priate safety, health, and environmental practices and deter-
4.4 Presser Foot, having a flat surface 0.395 6 0.02 in. (10
mine the applicability of regulatory limitations prior to use.
6 0.5 mm) in diameter, and can be lifted by a lever at least 13
1.4 This international standard was developed in accor-
mm or 0.5 in. It shall be dead-mass loaded to exert a total load
dance with internationally recognized principles on standard-
of 13.86 6 0.35 oz (393 6 10 g) on the specimen. The load is
ization established in the Decision on Principles for the 2
equivalent to 500 g/cm . The contacting surface of the presser
Development of International Standards, Guides and Recom-
foot and the surface of the anvil shall be parallel within 0.0001
mendations issued by the World Trade Organization Technical
in. (0.0025 mm).
Barriers to Trade (TBT) Committee.
5. Test Specimen
2. Referenced Documents
5.1 The test specimen shall be a piece of leather that has
2
2.1 ASTM Standards:
been conditioned according to Practice D1610 and cut to the
D1610 Practice for Conditioning Leather and Leather Prod-
dimensions required for the particular physical test.
ucts for Testing
6. Procedure
3. Significance and Use
6.1 Place the specimen on the anvil, and lower the presser
3.1 This test method shall be used where precise dimensions
footgently(donotdrop)untilitrestsonthespecimen.Takethe
are necessary for calculation of properties expressed in physi-
reading 5 s after the full load is reached. Read the thickness to
cal units. It is n
...

This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
Designation: D1813 − 13 D1813 − 13 (Reapproved 2017)
Standard Test Method for
1
Measuring Thickness of Leather Test Specimens
This standard is issued under the fixed designation D1813; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the U.S. Department of Defense.
1. Scope
1.1 This test method covers the measurement of the thickness of leather test specimens in which the dimensions of the
specimens are used directly in determining the results of tests for physical properties. This test method does not apply to wet blue.
1.2 The values stated in inch-pound units are to be regarded as standard. The values given in parentheses are mathematical
conversions to SI units that are provided for information only and are not considered standard.
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility
of the user of this standard to establish appropriate safety safety, health, and healthenvironmental practices and determine the
applicability of regulatory limitations prior to use.
1.4 This international standard was developed in accordance with internationally recognized principles on standardization
established in the Decision on Principles for the Development of International Standards, Guides and Recommendations issued
by the World Trade Organization Technical Barriers to Trade (TBT) Committee.
2. Referenced Documents
2
2.1 ASTM Standards:
D1610 Practice for Conditioning Leather and Leather Products for Testing
3. Significance and Use
3.1 This test method shall be used where precise dimensions are necessary for calculation of properties expressed in physical
units. It is not intended to replace practical thickness measurements based on commercial portable tools, nor is it implied that
thickness measurements made by the two procedures will agree exactly.
4. Apparatus
3
4.1 Gage, equipped with a dial micrometer, a flat anvil, and a presser foot loaded by a dead mass.
4.2 Dial, graduated to read to the nearest 0.01 mm, with small second dial graduated to read to the nearest 1 mm or to the nearest
0.001 in. and 0.1 in. respectively.
4.3 Anvil, flat, with a diameter of 0.395 6 0.02 in. (10 6 0.5 mm) and projecting 0.1 in. (2.5 mm) from the surface of a flat
circular platform about 2 in. (50 mm) in diameter.
4.4 Presser Foot, having a flat surface 0.395 6 0.02 in. (10 6 0.5 mm) in diameter, and can be lifted by a lever at least 13 mm
or 0.5 in. It shall be dead-mass loaded to exert a total load of 13.86 6 0.35 oz (393 6 10 g) on the specimen. The load is equivalent
2
to 500 g/cm . The contacting surface of the presser foot and the surface of the anvil shall be parallel within 0.0001 in. (0.0025 mm).
5. Test Specimen
5.1 The test specimen shall be a piece of leather that has been conditioned according to Practice D1610 and cut to the
dimensions required for the particular physical test.
1
This test method is under the jurisdiction of ASTM Comm
...

Questions, Comments and Discussion

Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.