Abstract

This document describes methods of evaluating the resistance of vulcanized and thermoplastic rubbers to the action of liquids by measurement of properties of the rubbers before and after immersion in test liquids. The liquids concerned include current service liquids, such as petroleum derivatives, organic solvents and chemical reagents, as well as reference test liquids.

Status
Published
Publication Date
11-Aug-2026
Current Stage
6060 - International Standard published - 60 Publication
Start Date
12-Aug-2026
Due Date
21-Jan-2027
Completion Date
21-Jan-2027

Buy Documents

Standard

ISO 1817:2026 - Rubber, vulcanized or thermoplastic — Determination of the effect of liquids

Release Date:12-Aug-2026
English language (30 pages)
sale 15% off
Preview
sale 15% off
Preview
Standard

ISO 1817:2026 - Caoutchouc vulcanisé ou thermoplastique — Détermination de l'action des liquides

Release Date:12-Aug-2026
French language (32 pages)
sale 15% off
Preview
sale 15% off
Preview

ISO 1817:2026 is an International Organization for Standardization (ISO) standard for testing vulcanized and thermoplastic rubber against liquids. It specifies how to measure property changes before and after immersion in service liquids or reference test liquids, so users can compare rubber compounds under controlled conditions. The tests are run on unstressed test pieces and are useful for comparative assessment and quality control, not for direct prediction of service behaviour.

What does ISO 1817:2026 specify?

ISO 1817:2026 specifies methods for evaluating the resistance of vulcanized and thermoplastic rubbers to liquids by measuring properties before and after immersion. The liquids include current service liquids such as petroleum derivatives, organic solvents and chemical reagents, as well as reference test liquids.

The document is organized into clauses for scope, references, apparatus, calibration, test liquids, test pieces, immersion conditions, procedures, precision and reporting. It also has three annexes that give reference liquids, calibration scheduling and precision data.

AnnexWhat it covers
Annex AReference liquids, including simulated fuels, reference oils, simulated service liquids, cooling lubricants and chemical reagents
Annex BCalibration schedule for the test apparatus
Annex CPrecision data from an interlaboratory test programme

The introduction also explains the purpose of the measurements: liquid action can cause absorption, extraction or chemical reaction, leading to swelling and changes in hardness, tensile properties and dimensions.

What are the key requirements of ISO 1817:2026?

ISO 1817:2026 requires the tester to choose a method, a liquid, a temperature and a duration that suit the intended use, then measure the relevant property changes on three test pieces. In practice, this makes the method adaptable, but it also means the test description and report must be specific enough for another laboratory to repeat the work.

Clause 4 - choose the right apparatus and method

Clause 4 defines five methods.

  • Method A uses a glass vessel with a glass lid and is suitable for non-volatile and volatile liquids below their boiling point.
  • Method B uses a closed glass vessel to reduce evaporation and air ingress.
  • Method C uses a reflux condenser and is intended for high-volatility liquids near boiling point.
  • Method D uses a pressure vessel for above-boiling or flammable liquids, or where evaporation and air contact must be fully prevented.
  • Method E exposes only one surface of the test piece, which is useful for sheet products such as diaphragms.

The practical point is that the vessel and sealing arrangement must match the liquid being tested. For example, volatile liquids need tighter control of evaporation, while one-sided exposure requires different fixtures.

Clause 5 and Annex B - calibrate the equipment

Clause 5 makes calibration mandatory and points to Annex B. Annex B gives a calibration schedule for the main apparatus and the measuring instruments.

This matters because the result depends on vessel volume, immersion geometry, balance accuracy and dimensional measurement. The balance must be accurate to 1 mg, and the measuring instruments for dimensions and surface area must meet the specified resolution.

Clause 6 and Annex A - select and characterize the test liquid

Clause 6 says the preferred test liquid is the actual service liquid, if possible. If a commercial liquid is used, the report should include enough detail to identify it, because composition can vary.

For mineral oils, the report must include density, refractive index, viscosity and aniline point or aromatic content. Annex A supplies defined reference liquids for simulated fuels, reference oils, simulated service liquids, metalworking fluids (MWFs) and chemical reagents. In practice, this gives a common basis for classification and quality control when the real service liquid is variable or unavailable.

Clause 7 - prepare and condition the test pieces

Clause 7 requires test pieces to be prepared in accordance with ISO 23529 and, where possible, to have a uniform thickness of (2 ± 0.2) mm. Different property measurements use different shapes and sizes, including dumb-bells, discs, quadrilateral pieces and rhomboid pieces.

The timing after vulcanization also matters. The standard sets minimum and maximum intervals, and test pieces in the “as received” condition must be conditioned at a standard laboratory temperature before testing. This helps laboratories compare results on similar thermal and ageing histories.

Clause 8 - control immersion temperature and duration

Clause 8 requires immersion at one or more standard laboratory temperatures unless otherwise specified. It also notes that higher temperatures can increase oxidation, volatilization and decomposition, so the temperature choice affects the result.

The immersion time depends on the liquid and the rubber. The standard recommends repeated measurements for acceptance work and a single suitable period for control work. The practical meaning is that users should record how the property changes with time, not just one end point.

Clause 9 - measure the property changes

Clause 9 covers the core measurements:

  • change in mass
  • change in volume
  • change in dimensions
  • change in surface area
  • change in hardness
  • change in tensile stress-strain properties
  • one-surface exposure
  • extractable matter

The standard gives calculation formulas for each property. It also states that results are reported as the median of three test pieces. That reduces the influence of individual sample variation.

For hardness, the document uses micro International Rubber Hardness Degree (IRHD) from ISO 48-2, with an alternative mention of ISO 48-4 in a note. For tensile properties, it refers to ISO 37. For extractable matter, it gives two options: weigh the dried test piece or evaporate the test liquid and weigh the residue.

Clause 11 - report enough detail to repeat the test

Clause 11 requires the report to identify the sample, the preparation method, the method used, the test piece type and dimensions, the liquid, the temperature, conditioning, immersion period, any liquid replacement and any deviation from the procedure. It also requires the results, the appearance of the test piece or liquid when relevant, and the test date.

Who uses ISO 1817:2026?

ISO 1817:2026 is used by rubber testing laboratories, compounders, quality control teams, product developers and buyers who need to compare rubber resistance to oils, fuels, solvents, reagents or process fluids. It is relevant for seals, hoses, diaphragms, molded parts and other rubber products that contact liquids in service.

It is also used when qualifying new compounds, checking batch consistency, or investigating whether a product is suitable for a particular liquid exposure. The reference liquids in Annex A make it useful for classification work and routine comparison testing.

What changed in ISO 1817:2026 from the previous edition?

ISO 1817:2026 cancels and replaces ISO 1817:2024. The foreword states that this ninth edition has been technically revised, and the stated change is that Clause 4 now allows water baths, oil baths or heat blocks for method B.

Which standards are used with ISO 1817:2026?

ISO 1817:2026 refers to these standards and related documents:

  • ISO 37 - tensile stress-strain testing for rubber, used in Clause 9.8.
  • ISO 48-2 - micro IRHD hardness, used in Clause 9.7.
  • ISO 18899 and ISO 18899:2013 - calibration guidance for test equipment, used in Clause 5 and Annex B.
  • ISO 23529 - preparation and conditioning of test pieces, and apparatus requirements for some instruments.
  • ASTM D5964-16 - specifications for the reference oils in Annex A.
  • ISO/TR 9272 and ISO 19983 - precision concepts and calculations referenced in Annex C.
  • ISO 175 - cited in Annex A as a useful list of chemical reagents when no product-specific specification is known.
  • ISO 48-4 - cited in a note as an alternative hardness method.

What does the ISO 1817:2026 document contain?

ISO 1817:2026 contains apparatus descriptions for five immersion methods, including examples shown in Figures 1 to 7. It gives formulas for calculating percentage changes in mass, volume, dimensions, surface area, hardness, tensile properties and extractable matter.

Annex A provides reference liquid recipes and descriptions, including simulated fuels, reference oils, simulated service liquids and MWF formulations. Annex B gives a calibration schedule in table form, and Annex C reports precision results from an interlaboratory test programme, with tables for repeatability and reproducibility across different properties and exposure conditions.

Relations

Effective Date
25-Jan-2025

Buy Documents

Standard

ISO 1817:2026 - Rubber, vulcanized or thermoplastic — Determination of the effect of liquids

Release Date:12-Aug-2026
English language (30 pages)
sale 15% off
Preview
sale 15% off
Preview
Standard

ISO 1817:2026 - Caoutchouc vulcanisé ou thermoplastique — Détermination de l'action des liquides

Release Date:12-Aug-2026
French language (32 pages)
sale 15% off
Preview
sale 15% off
Preview

Get Certified

Connect with accredited certification bodies for this standard

DIN CERTCO

DIN Group product certification.

DAKKS Germany Verified

Smithers Quality Assessments

US management systems and product certification.

ANAB United States Verified

Sponsored listings

Frequently Asked Questions

ISO 1817:2026 is a standard published by the International Organization for Standardization (ISO). Its full title is "Rubber, vulcanized or thermoplastic — Determination of the effect of liquids". This standard covers: This document describes methods of evaluating the resistance of vulcanized and thermoplastic rubbers to the action of liquids by measurement of properties of the rubbers before and after immersion in test liquids. The liquids concerned include current service liquids, such as petroleum derivatives, organic solvents and chemical reagents, as well as reference test liquids.

This document describes methods of evaluating the resistance of vulcanized and thermoplastic rubbers to the action of liquids by measurement of properties of the rubbers before and after immersion in test liquids. The liquids concerned include current service liquids, such as petroleum derivatives, organic solvents and chemical reagents, as well as reference test liquids.

ISO 1817:2026 is classified under the following ICS (International Classification for Standards) categories: 83.060 - Rubber. The ICS classification helps identify the subject area and facilitates finding related standards.

ISO 1817:2026 has the following relationships with other standards: It is inter standard links to ISO 1817:2024. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.

ISO 1817:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)

Contents

  • Introduction
  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 4 Apparatus
  • 4.1 General
  • 4.2 Apparatus for method A
  • 4.3 Apparatus for method B
  • 4.4 Apparatus for method C
  • 4.5 Apparatus for method D
  • 4.6 Apparatus for method E
  • 4.7 Additional equipment
  • 5 Calibration
  • 6 Test liquids
  • 7 Test pieces
  • 7.1 Preparation
  • 7.2 Dimensions
  • 7.3 Time interval between vulcanization and testing
  • 7.4 Conditioning
  • 8 Immersion in the test liquid
  • 8.1 Temperature
  • 8.2 Duration
  • 9 Procedure
  • 9.1 General
  • 9.2 Replacement of test liquid
  • 9.3 Change in mass
  • 9.4 Change in volume
  • 9.5 Change in dimensions
  • 9.6 Change in surface area
  • 9.7 Change in hardness
  • 9.8 Change in tensile stress-strain properties
  • 9.9 Testing with liquid on one surface only
  • 9.10 Determination of extractable matter
  • 10 Precision
  • 11 Test report
  • Annex A
  • Annex B
  • 19.1 U Method B
  • Annex C
  • Bibliography

Introduction

The action of a liquid on vulcanized or thermoplastic rubber can generally result in:

a) absorption of the liquid by the rubber; b) extraction of soluble constituents from the rubber; c) a chemical reaction with the rubber.

The amount of absorption [a)] is usually larger than that of extraction [b)], so that the net result is an increase in volume, commonly termed “swelling”. The absorption of liquid can profoundly alter physical and chemical properties and hence change tensile strength, extensibility and hardness of the rubber, so it is important to measure these properties after treatment of the rubber. The extraction of soluble constituents, especially plasticizers and antidegradants can likewise alter the rubber's physical properties and chemical resistance after drying (assuming the liquid to be volatile). Therefore, it is necessary to test these properties following immersion and drying of the rubber. This document describes the methods necessary for determining the following properties after immersion and after immersion and drying:

  • change in mass, volume and dimensions;
  • extractable matter;
  • change in hardness and tensile stress-strain properties.

Although in some respects these tests can simulate service conditions, no direct correlation with service behaviour is implied. Thus, the rubber giving the lowest change in volume is not necessarily the best one in service. The thickness of the rubber must be taken into account, since the rate of penetration of liquid is time-dependent and the bulk of a very thick rubber product can remain unaffected for the whole of the projected service life, especially with viscous liquids. Moreover, it is known that the action of a liquid on rubber, especially at high temperatures, can be affected by the presence of atmospheric oxygen. The tests described in this document can, however, provide valuable information on the suitability of a rubber for use with a given liquid and, in particular, constitute a useful control when used for developing rubbers resistant to oils, fuels or other service liquids.

The effect of a liquid can depend on the nature and magnitude of any stress within the rubber. In this document, test pieces are tested in an unstressed condition.

International Standard ISO 1817:2026(en) Rubber, vulcanized or thermoplastic — Determination of the effect of liquids

1 Scope

This document describes methods of evaluating the resistance of vulcanized and thermoplastic rubbers to the action of liquids by measurement of properties of the rubbers before and after immersion in test liquids. The liquids concerned include current service liquids, such as petroleum derivatives, organic solvents and chemical reagents, as well as reference test liquids.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 37, Rubber, vulcanized or thermoplastic — Determination of tensile stress-strain properties ISO 48-2, Rubber, vulcanized or thermoplastic — Determination of hardness — Part 2: Hardness between 10 IRHD and 100 IRHD ISO 18899:2013, Rubber — Guide to the calibration of test equipment ISO 18899, Rubber — Guide to the calibration of test equipment ISO 23529, Rubber — General procedures for preparing and conditioning test pieces for physical test methods ASTM D5964-16, Standard Practice for Rubber IRM 901, IRM 902, and IRM 903 Replacement Oils for ASTM No. 1, ASTM No. 2, ASTM No. 3 Oils, and IRM 905 formerly ASTM No. 5 Oil

3 Terms and definitions

No terms and definitions are listed in this document.

ISO and IEC maintain terminology databases for use in standardization at the following addresses:

  • ISO Online browsing platform: available at https:// www .iso .org/ obp
  • IEC Electropedia: available at https:// www .electropedia .org/

4 Apparatus

4.1 General

WARNING — Persons using this document should be familiar with normal laboratory practice. This document does not purport to address all of the safety problems, if any, associated with its use. It is the responsibility of the user to establish appropriate safety and health practices and to determine the applicability of any other restrictions.

WARNING — Certain procedures specified in this document can involve the use or generation of substances, or the generation of waste, that could constitute a local environmental hazard. Reference should be made to appropriate documentation on safe handling and disposal after use.

ISO 1817:2026(en) Five different methods are defined, all with different equipment. Method A – Glass vessel with glass lid. Suitable for test with non-volatile and volatile liquids, below the boiling point. Examples of non-volatile liquids are different type of oils (mineral or synthetic), for example engine, gearbox and hydraulic oils.

Method B – Glass vessel with stopper or lid, in order to prevent and minimize evaporation of the test liquid and the ingress of air. Suitable for test with non-volatile and volatile liquids, below the boiling point. Method C – Glass vessel with reflux condenser. For test with high volatile liquids, near the boiling point. Method D – Pressure vessel with hermetically closed lid, allowing for test at overpressure. For test, for example, above the boiling point, with flammable liquids, or where evaporation of the liquid and ingress of air shall be completely hindered.

Method E – Apparatus for testing one surface only.

In method A, the liquid to test piece volume ratio shall be (80 ± 10):1 and the amount of air above the liquid shall be 10 % ± 2 % of the total vessel volume. If the test deviates from this, it shall be clearly stated in the report. This means that the size of the vessel depends on the size and the amount of test pieces to be tested. In methods B to D, the volume of liquid shall be at least 15 times the combined volume of the test pieces and the volume of air above the liquid shall be kept to a minimum. The test pieces in methods A to D shall be mounted hanging on a rod or wire and separated from any adjacent test piece. For a greater number of test pieces, use of a test piece holder can be useful. A possible test piece holder preventing the contact and the floating of samples with lower density is shown in Figure 1 and Figure 2.

The materials of the hanger, as well as of the apparatus, shall be inert to the test liquid and to the rubber; for example, materials containing copper shall not be used.

Stirring of the liquid is not permitted except in method C.

Heating of the vessels shall be done by storing the vessel in an air heated oven, except for method C where a heating mantle is recommended. For method B also water baths, oil baths or heating blocks are allowed to use.

Example on apparatus for methods A to D are shown in Figure 1 to Figure 7.

4.2 Apparatus for method A

The glass vessel shall be of flange type with ground surface. The lid shall have a ground surface where it seals to the vessel flange and shall be clamped by suitable means, for example by a wire or steel bracket. The size of the vessel shall be so that the liquid to test piece volume ratio is (80 ± 10):1. Greasing or use of rubber sealant on the flanges is not permitted.

Measurements need to be taken in order to avoid sticking of test pieces in a vessel (shown in Figure 3).

ISO 1817:2026(en) Figure 1 — Example of test piece rack with trays and test pieces (type 2 dumbbells and discs) Figure 2 — Example of tray and tray-weight for test pieces with low density Figure 3 — Example of glass vessel with lid and inside oven

ISO 1817:2026(en) For pressure relief, if the vessel is closed with a glass stopper it can be necessary to open this shortly after the desired temperature is stable inside the oven (vessel).

4.3 Apparatus for method B

A glass vessel with stopper or lid shall be used to prevent the ingress of air.

4.4 Apparatus for method C

4.4.1 General

A glass vessel fitted with a reflux condenser shall be used.

Vessel usually heated up on a heating plate with a magnetic stirrer.

4.4.2 With air contact

Figure 4 gives an example configuration of a reflux condenser and, if necessary, additional openings to have contact to the atmosphere so that a contact of air or oxygen is possible via the surface of the test liquid. Figure 4 — Example configuration of reflux condenser with air contact

4.4.3 Without air contact

To prevent air (oxygen) contact with the atmosphere, it is possible to connect the reflux condenser with two bottles with a separation liquid. The liquid should not react or generate volatiles which can react with the test liquid. This is shown in Figure 5.

ISO 1817:2026(en) Figure 5 — Example reflux condenser to prevent air (oxygen) contact with the atmosphere.

4.5 Apparatus for method D

A pressure vessel of suitable quality for the liquid to be tested shall be used. The lid shall be hermetically closed by a suitable type of sealing and clamping. The vessel shall be designed to withstand the temperature and pressure it will be exposed to. In Figure 6 (4) an example of such a vessel is shown.

ISO 1817:2026(en) Key 1 method A 2 method B 3 method C 4 method D Figure 6 — Possible apparatus for methods A to D

4.6 Apparatus for method E

An apparatus for testing one surface only, which holds the test piece in contact with the liquid on only one of its surfaces, shall be used.

A suitable apparatus is illustrated in Figure 7. It comprises a base-plate (A) and an open-ended cylindrical chamber (B), which is held tightly against the test piece (C) by wing nuts (D) mounted on bolts (E). A hole of approximately 30 mm diameter is allowed in the base-plate for examination of the surface not in contact with the liquid. During the test, the opening on the top of the chamber shall be closed by a close-fitting plug (F).

ISO 1817:2026(en) Dimensions in millimetres Key A base plate B open-ended cylindrical chamber C test piece D wing nuts E bolts F close fitting plug Figure 7 — Apparatus for method E (testing one surface only)

4.7 Additional equipment

4.7.1 Balance, accurate to 1 mg.

4.7.2 Instrument for measuring the thickness of the test piece, consisting of a micrometre dial gauge, of adequate accuracy, firmly held in a rigid stand over a flat base-plate. The instrument shall conform to the requirements given for such apparatus in ISO 23529.

4.7.3 Instrument for measuring the length and width of the test piece, having a scale graduated in divisions of 0,01 mm and preferably operating without contact with the test piece, for example using an optical system conforming to the requirements given for such apparatus in ISO 23529. 4.7.4 Instrument for measuring the change in surface area, capable of measuring the lengths of the diagonals of the test piece. It shall have a scale graduated in divisions of 0,01 mm and should preferably operate without contact with the test piece, for example using an optical system conforming to the requirements given for such apparatus in ISO 23529.

5 Calibration

The test apparatus shall be calibrated in accordance with the requirements in Annex B.

ISO 1817:2026(en)

6 Test liquids

The choice of the test liquid shall depend on the purpose of the test. When information is required on the service behaviour of a vulcanized or thermoplastic rubber in contact with a particular liquid, then this liquid shall, if possible, be chosen for the test. Commercial liquids are not always constant in composition, and the test shall, whenever practicable, include a reference material of known characteristics. Any abnormal results due to unexpected variations in the composition of the commercial liquid will thus become apparent. It can then be necessary to set aside a bulk supply of the liquid for a particular series of tests.

Mineral oils and fuels are liable to vary considerably in chemical composition even when supplied at a recognized specification. The aniline point of a mineral oil gives some indication of its aromatic content and helps to characterize the action of the oil on rubber, but the aniline point alone is not sufficient to characterize a mineral oil; other things being equal, the lower the aniline point, the more pronounced the action. If a mineral oil is used as test liquid, the test report shall include the density, refractive index, viscosity and aniline point or aromatic content of the oil.

Service oils having similar fluid characteristics to the reference liquids (see Clause A.1 to Clause A.3) will not necessarily have the same effect on the material as the reference liquids. Some fuels, particularly gasoline, vary widely in composition and, for some possible constituents, minor variations can have a large influence on the effect on rubber. Complete details of the composition of the fuel used shall therefore be included in the test report.

Metalworking fluids (MWFs) or Cooling Lubricants are used in workshops worldwide for the cutting and forming of metals. Their main purposes are to cool and lubricate tools, work pieces and machines, inhibit corrosion and remove swarf. MWFs are available as non-water-miscible oils, water-miscible or emulsifiable concentrates or fully synthetic, oil-free products. Non-water-miscible MWFs mainly consist of base oil (usually over 95 %). This can be a mineral oil, ester oil (e.g. unrefined or chemically modified rapeseed oil) or synthetic oil (e.g. poly-alpha-olefin). For testing, they can be used as they are shipped. Water-miscible MWFs are mixed with water before use, in concentrations of 2 % to 25 %, depending on the product and type of machining. This type of MWF is based on oil and shares of 20 % to 80 % are possible. To combine this oil with water to yield an oil-in-water emulsion, an emulsifier is necessary. Fully and semisynthetic fluids types of MWFs are water-miscible and do not require emulsifiers. They can be based on water-miscible glycol compounds, for example. Mixing in water yields a transparent water-mixed MWF. Seal compatibility tests can be performed either with the delivered concentrate or fresh prepared emulsion or solution. For mixing a test emulsion or solution, de-ionized water at ambient temperature should be used. The standard concentration is a mass fraction of 10 %, but other concentrations can be used if necessary. The metalworking fluid concentrate should be added slowly to water with agitation (e.g. by employing a magnetic stirrer), to avoid gelling or splitting of the emulsion. As commercial liquids do not always have a constant composition, a standard liquid consisting of welldefined chemical compounds or mixtures of compounds, in accordance with Annex A, shall be used as reference liquid for the purpose of classification of vulcanized or thermoplastic rubbers or quality control. When testing to determine the effect of chemical solutions, the concentration of the solution shall be appropriate to the intended use.

Depending on the temperature, the composition of the test liquid can change significantly during immersion. The ageing of the test liquid and any interaction with the test pieces shall be taken into consideration. If there are chemically active additives in the liquid, or if there is a significant change in composition by extraction, absorption or reaction with the rubber, either the volume shall be increased or the liquid shall be replaced with fresh liquid at specified intervals. See 9.2 for more information. Some liquids are sensitive to oxidation. Thus, they will change significantly when exposed to air at elevated temperature, which can be the case in Method C.

NOTE It has been shown that when using commercial oils containing additives, it is not only important to prevent the entry of air, but also the escape of volatiles from the immersion vessel (degradation products of the oil or its additives can be very aggressive).

ISO 1817:2026(en)

7 Test pieces

7.1 Preparation

Test pieces shall be prepared in accordance with ISO 23529.

7.2 Dimensions

Data obtained on test pieces having different original thicknesses are not always comparable. Therefore, where possible, test pieces shall be of uniform thickness of (2 ± 0,2) mm. Test pieces cut from commercial articles may be used. For products thinner than 1,8 mm, use the original thickness. If the material is thicker than 2,2 mm, reduce the thickness to (2 ± 0,2) mm (see ISO 23529). 3 3 Test pieces for the determination of the change in volume and mass shall have a volume of 1 cm to 3 cm . Test pieces for the determination of the change in hardness shall have lateral dimensions of no less than 8 mm.

Test pieces for the determination of the change in dimensions shall be quadrilateral with sides between 25 mm and 50 mm in length, or circular with a diameter of 44,6 mm (internal diameter of type A test piece in ISO 37). This type of test piece can also be used for the determination of mass and volume. Test pieces for the determination of the change in surface area shall be rhomboid, with the sides cut cleanly and at right angles to the top and bottom surfaces. This can be achieved by two consecutive cuts at approximately right angles to each other, with a cutter consisting of two parallel blades, suitably spaced. The length of the sides shall be nominally 8 mm. Circular test pieces with a diameter of 44,6 mm can also be used.

NOTE For the determination of the change in surface area, it can be convenient to use smaller or thinner test pieces, for example when cut from products or when rapid attainment of equilibrium is required. However, the results can differ from those obtained using the specified thickness. Smaller test pieces will reduce the precision of the results.

Test pieces for the determination of tensile properties shall be in accordance with ISO 37. Type 2 dumb-bells are preferred because their size makes them more convenient to immerse in liquid than type 1. The type 2 test piece can also be used when determining the change in mass, volume or hardness. For tests with liquid contact on one surface only, the test piece shall consist of a disc with a diameter of about 60 mm.

7.3 Time interval between vulcanization and testing

Unless otherwise specified for technical reasons, the following requirements, in accordance with ISO 23529 for time intervals, shall be observed.

For all test purposes, the minimum time between vulcanization and testing shall be 16 h. For non-product tests, the maximum time between vulcanization and testing shall be 4 weeks and, for evaluations intended to be comparable, the tests shall be carried out using, as far as possible, the same time interval.

For product tests, whenever possible, the time between vulcanization and testing shall not exceed 3 months. In other cases, tests shall be made within 2 months of the date of receipt of the product by the customer.

7.4 Conditioning

Test pieces for test in the “as received” condition shall be conditioned for not less than 3 h at one of the standard laboratory temperatures specified in ISO 23529. The same temperature shall be used throughout any test or any series of tests intended to be comparable.

ISO 1817:2026(en)

8 Immersion in the test liquid

8.1 Temperature

Unless otherwise specified, the immersion shall be carried out at one or more of the temperatures listed in ISO 23529.

...

Contents

  • Introduction
  • 1 Domaine d’application
  • 2 Références normatives
  • 3 Termes et définitions
  • 4 Appareillage
  • 4.1 Généralités
  • 4.2 Appareillage pour la méthode A
  • 4.3 Appareillage pour la méthode B
  • 4.4 Appareillage pour la méthode C
  • 4.5 Appareillage pour la méthode D
  • 4.6 Appareillage pour la méthode E
  • 4.7 Equipement supplémentaire
  • 5 Étalonnage
  • 6 Liquides d’essai
  • 7 Éprouvettes
  • 7.1 Préparation
  • 7.2 Dimensions
  • 7.3 Délai entre vulcanisation et essai
  • 7.4 Conditionnement
  • 8 Immersion dans le liquide d’essai
  • 8.1 Température
  • 8.2 Durée
  • 9 Mode opératoire
  • 9.1 Généralités
  • 9.2 Remplacement de liquide d’essai
  • 9.3 Variation de masse
  • 9.4 Variation de volume
  • 9.5 Variation de dimensions
  • 9.6 Variation de surface
  • 9.7 Variation de dureté
  • 9.8 Variation des propriétés de résistance à la contrainte-déformation
  • 9.9 Essai avec un liquide sur une seule face
  • 9.10 Détermination des matières solubles extraites
  • 10 Fidélité
  • 11 Rapport d'essai
  • Annexe A
  • Annexe B
  • 19.1 U Méthode B
  • Annexe A
  • Annexe C
  • Bibliographie

Introduction

En général, l’action d’un liquide sur un caoutchouc vulcanisé ou thermoplastique peut conduire à:

a) l’absorption du liquide par le caoutchouc; b) l’extraction des constituants solubles du caoutchouc; c) une réaction chimique avec le caoutchouc.

En général, il se produit davantage d’absorption [a)] que d’extraction [b)], de sorte que le résultat final est un accroissement en volume, habituellement appelé “gonflement”. L’absorption de liquide peut modifier profondément les propriétés physiques et chimiques du caoutchouc et, par conséquent, sa résistance, son allongement à la traction et sa dureté, de sorte qu’il est important de mesurer ces propriétés du caoutchouc après traitement. L’extraction des constituants solubles, en particulier celle des plastifiants et des agents de protection peut également modifier les propriétés physiques et chimiques du caoutchouc après évaporation du liquide (en supposant que celui-ci soit volatil). C’est pourquoi les essais physiques du caoutchouc sont requis après immersion et séchage. Le présent document décrit les méthodes nécessaires pour la détermination des propriétés suivantes après immersion et après immersion et séchage:

  • variation de masse, de volume et de dimensions;
  • matières solubles extraites;
  • variation des propriétés de contrainte-déformation en traction et de dureté. Bien qu’à certains égards, ces essais puissent simuler les conditions de service, il n’y a pas de corrélation directe entre les résultats d’essai et la tenue en service du vulcanisat. Ainsi, le caoutchouc donnant la plus faible variation de volume n’est pas nécessairement le meilleur en service. Il est nécessaire de prendre en considération l’épaisseur du caoutchouc étant donné que le taux de pénétration du liquide d’essai dépend du temps d’immersion et qu’un produit en caoutchouc très épais peut rester inchangé “à cœur” pendant toute sa durée de service, notamment avec des liquides visqueux. De plus, il s’est avéré que l’action d’un liquide sur le caoutchouc, particulièrement à haute température, peut être affectée par la présence d’oxygène atmosphérique. Cependant, les essais décrits dans le présent document peuvent fournir des renseignements précieux sur l’aptitude à l’emploi d’un caoutchouc en présence d’un liquide donné et, en particulier, constituent un moyen de contrôle utile lors de la mise au point de caoutchoucs résistants aux huiles, aux combustibles ou à d’autres liquides.

L'effet d'un liquide peut dépendre de la nature et de l'importance des contraintes que subit le caoutchouc. Dans le présent document, les éprouvettes sont soumises à essai sans contrainte appliquée.

Norme internationale ISO 1817:2026(fr) Caoutchouc vulcanisé ou thermoplastique — Détermination de l'action des liquides

1 Domaine d’application

Le présent document spécifie des méthodes pour évaluer la résistance des caoutchoucs vulcanisés ou thermoplastiques à l’action des liquides, par mesurage de leurs caractéristiques avant et après immersion dans des liquides d’essai. Les liquides considérés comprennent des liquides de service tels que des dérivés du pétrole, des solvants organiques et des réactifs chimiques ainsi que des liquides d’essai de référence.

2 Références normatives

Les documents suivants sont cités dans le texte de sorte qu’ils constituent, pour tout ou partie de leur contenu, des exigences du présent document. Pour les références datées, seule l’édition citée s’applique. Pour les références non datées, la dernière édition du document de référence s'applique (y compris les éventuels amendements).

ISO 37, Caoutchouc vulcanisé ou thermoplastique — Détermination des caractéristiques de contraintedéformation en traction ISO 48-2, Caoutchouc vulcanisé ou thermoplastique — Détermination de la dureté — Partie 2: Dureté comprise entre 10 DIDC et 100 DIDC ISO 18899:2013, Caoutchouc — Guide pour l’étalonnage du matériel d’essai ISO 18899, Caoutchouc — Guide pour l’étalonnage du matériel d’essai ISO 23529, Caoutchouc — Procédures générales pour la préparation et le conditionnement des éprouvettes pour les méthodes d’essais physiques ASTM D5964, Standard Practice for Rubber IRM 901, IRM 902, and IRM 903 Replacement Oils for ASTM No. 1, ASTM No. 2, ASTM No. 3 Oils, and IRM 905 formerly ASTM No. 5 Oil

3 Termes et définitions

Aucun terme n’est défini dans le présent document.

L’ISO et l’IEC tiennent à jour des bases de données terminologiques destinées à être utilisées en normalisation, consultables aux adresses suivantes:

  • ISO Online browsing platform: disponible à l’adresse https:// www .iso .org/ obp
  • IEC Electropedia: disponible à l’adresse https:// www .electropedia .org/

4 Appareillage

4.1 Généralités

AVERTISSEMENT — Il convient que les utilisateurs du présent document soient familiarisés avec les pratiques normales de laboratoire. Le présent document ne prétend pas traiter de tous les problèmes de sécurité, le cas échéant, liés à son utilisation. Il incombe à l’utilisateur d’établir des

ISO 1817:2026(fr) pratiques appropriées en matière de sécurité et de santé et de déterminer l’applicabilité de toute autre restriction.

AVERTISSEMENT — Certaines procédures spécifiées dans le présent document peuvent impliquer l’utilisation ou la génération de substances, ou la production de déchets, susceptibles de constituer un danger pour l’environnement local. Il convient de se référer à la documentation appropriée concernant la manipulation en toute sécurité et l’élimination après utilisation. Cinq méthodes différentes sont définies, toutes avec des équipements différents. Méthode A – Récipient en verre avec couvercle en verre. Approprié pour les essais avec des liquides non volatils et volatils, en dessous du point d'ébullition. Des exemples de liquides non volatils sont différents types d'huiles (minérales ou synthétiques), par exemple les huiles pour moteur, pour boîte de vitesses et les huiles hydrauliques.

Méthode B – Récipient en verre avec bouchon ou couvercle, afin d’éviter et de réduire au minimum l’évaporation du liquide d’essai et la pénétration de l’air. Approprié pour les essais avec des liquides non volatils et volatils, en dessous du point d'ébullition.

Méthode C – Récipient en verre avec réfrigérant à reflux. Pour les essais avec des liquides très volatils, proches du point d'ébullition.

Méthode D – Récipient sous pression avec couvercle hermétiquement fermé, permettant un essai en surpression. Pour les essais, par exemple, au-dessus du point d'ébullition, avec des liquides inflammables, ou lorsque l'évaporation du liquide et la pénétration de l'air doivent être complètement bloquées. Méthode E – Appareillage pour essai sur une seule face.

Dans la méthode A, le rapport entre le volume du liquide et celui de l'éprouvette doit être de (80 ± 10):1 et la quantité d'air au-dessus du liquide doit être égale à 10 % ± 2 % du volume total du récipient. Si l'essai s'en écarte, cela doit être clairement indiqué dans le rapport. Cela signifie que la taille du récipient dépend de la taille et de la quantité d'éprouvettes à soumettre à essai.

Dans les méthodes B à D, le volume du liquide doit être au moins égal à 15 fois le volume total des éprouvettes et le volume d'air au-dessus du liquide doit être maintenu à un niveau minimal. Dans les méthodes A à D, les éprouvettes doivent être suspendues à une tige ou à un fil, et séparées de l’éprouvette adjacente. Pour un plus grand nombre d'éprouvettes, l'utilisation d'un support d'éprouvette peut s'avérer utile. Un support d'éprouvette possible empêchant le contact et le flottement d'échantillons de faible densité est présenté à la Figure 1 et la Figure 2.

Les matériaux du support, ainsi que de l’appareillage, doivent être inertes vis-à-vis du liquide d’essai et du caoutchouc; par exemple des matériaux contenant du cuivre ne doivent pas être utilisés. L'agitation du liquide n'est pas autorisée, sauf dans la méthode C. Le chauffage des récipients doit être réalisé en stockant le récipient dans une étuve à air chaud, sauf pour la méthode C où un chauffe-ballon est recommandé. Pour la méthode B l'utilisation de bains d'eau, bains d'huile ou corps de chauffe est également possible.

Des exemples d’appareillage pour les méthodes A à D sont représentés à la Figure 1 à la Figure 7.

4.2 Appareillage pour la méthode A

Le récipient en verre doit être de type à bride avec une surface rectifiée. Le couvercle doit avoir une surface rectifiée là où il ferme hermétiquement le récipient, et doit être fixé par des moyens appropriés, par exemple par un fil métallique ou un étrier en acier. La taille du récipient doit être telle que le rapport entre le volume du liquide et celui de l'éprouvette est de (80 ± 10):1. Le graissage ou l'utilisation d'un produit d'étanchéité en caoutchouc sur les brides n'est pas autorisé.

Des mesures doivent être prises pour éviter que les éprouvettes ne collent au récipient (illustré à la Figure 3).

ISO 1817:2026(fr) Figure 1 — Exemple de support d'éprouvettes avec plateaux et éprouvettes (éprouvettes haltère de type 2 et disques) Figure 2 — Exemple de plateau et de poids de plateau pour des éprouvettes de faible densité

ISO 1817:2026(fr) Figure 3 — Exemple de récipient en verre avec couvercle et étuve intérieure Si le récipient est fermé par un bouchon de verre il peut être nécessaire de l'ouvrir brièvement pour réduire la pression une fois que la température souhaitée est stable à l'intérieur de l'étuve (récipient).

4.3 Appareillage pour la méthode B

Un récipient en verre avec bouchon ou couvercle doit être utilisé pour empêcher la pénétration de l'air.

4.4 Appareillage pour la méthode C

4.4.1 Généralités

Un récipient en verre avec réfrigérant à reflux doit être utilisé. Le récipient est généralement chauffé sur une plaque chauffante avec un agitateur magnétique.

4.4.2 En contact avec l'air

La Figure 4 donne un exemple de configuration d'un réfrigérant à reflux et, si nécessaire, d'ouvertures supplémentaires pour être en contact avec l'atmosphère, de sorte qu'un contact air ou oxygène soit possible via la surface du liquide d’essai.

ISO 1817:2026(fr) Figure 4 — Exemple de configuration d'un réfrigérant à reflux en contact avec l'air

4.4.3 Sans contact avec l’air

Pour éviter le contact de l'air (oxygène) avec l'atmosphère, il est possible de raccorder le réfrigérant à reflux à deux bouteilles contenant un liquide de séparation. Il convient que le liquide ne réagisse pas ou ne génère pas de substances volatiles susceptibles de réagir avec le liquide d'essai. Cela est illustré à la Figure 5.

ISO 1817:2026(fr) Figure 5 — Exemple de réfrigérant à reflux pour éviter le contact de l'air (oxygène) avec l'atmosphère

4.5 Appareillage pour la méthode D

Un récipient sous pression de qualité appropriée pour le liquide à soumettre à essai doit être utilisé. Le couvercle doit être fermé hermétiquement par un type d'étanchéité et de serrage approprié. Le récipient doit être conçu pour résister à la température et à la pression auxquelles il sera exposé. Un exemple d’un tel récipient est illustré à la Figure 6 (4).

ISO 1817:2026(fr) Légende 1 méthode A 2 méthode B 3 méthode C 4 méthode D Figure 6 — Appareillage possible pour les méthodes A à D

4.6 Appareillage pour la méthode E

Un appareillage pour essai sur une seule face, qui maintient l’éprouvette en contact avec le liquide sur une seule de ses faces, doit être utilisé.

Un appareil approprié est représenté à la Figure 7. Il comprend un socle plan (A), une chambre cylindrique (B) avec une extrémité ouverte maintenue fermement contre l’éprouvette (C) par des écrous papillons (D) montés sur les boulons (E). Une ouverture d’environ 30 mm de diamètre peut être ménagée dans le socle plan pour examiner la surface qui n’est pas en contact avec le liquide. Pendant l’essai, l’ouverture située dans la partie supérieure de la chambre doit être fermée au moyen d’un bouchon étanche (F).

ISO 1817:2026(fr) Dimensions en millimètres Légende A socle plan B chambre cylindrique avec une extrémité ouverte C éprouvette D écrous papillons E boulons F bouchon étanche Figure 7 — Appareillage pour la méthode E (essai sur une seule face)

4.7 Equipement supplémentaire

4.7.1 Balance, précise à 1 mg.

4.7.2 Appareil pour mesurer l’épaisseur de l’éprouvette, constitué d’un comparateur à cadran

d'exactitude appropriée, maintenu fermement dans un support rigide sur un socle plan. L’instrument doit être conforme aux exigences données pour cet appareillage dans l’ISO 23529. 4.7.3 Appareil pour mesurer la longueur et la largeur de l’éprouvette, gradué en divisions de 0,01 mm et opérant de préférence sans contact avec l’éprouvette, par exemple avec un système optique conforme aux exigences données pour cet appareillage dans l’ISO 23529.

4.7.4 Appareil pour mesurer la variation de surface, capable de mesurer les longueurs des diagonales de l’éprouvette. Il doit être gradué en divisions de 0,01 mm et il convient qu'il opère de préférence sans contact avec l’éprouvette, par exemple avec un système optique conforme aux exigences données pour cet appareillage dans l’ISO 23529.

5 Étalonnage

L’appareillage d’essai doit être étalonné; conformément aux exigences de l’Annexe B.

ISO 1817:2026(fr)

6 Liquides d’essai

Le choix du liquide d’essai doit dépendre de l’objectif de l’essai. Lorsque l’on désire obtenir des renseignements sur le comportement en service d’un caoutchouc vulcanisé au contact d’un liquide déterminé, c’est ce liquide qui, en principe, doit être utilisé pour l’essai. Toutefois, les liquides commerciaux n’ont pas toujours une composition constante et l’essai doit donc, chaque fois que possible, être effectué également sur un caoutchouc de référence de caractéristiques connues. Tous résultats anormaux dus à des variations imprévues de la composition des liquides commerciaux seront ainsi mis en évidence. II peut se révéler nécessaire de prévoir un volume de liquide suffisant pour une série déterminée d’essais.

Les huiles minérales et les carburants sont sujets à des variations appréciables de composition chimique, même s’ils répondent à une spécification reconnue. Le point d’aniline d’une huile minérale donne une indication sur sa teneur en aromatiques et aide à caractériser l’action de l’huile sur le caoutchouc, bien que le point d’aniline seul ne soit pas suffisant pour caractériser une huile minérale; toutes choses égales par ailleurs, l’action d’une huile est d’autant plus sévère que le point d’aniline est plus bas. Si une huile minérale est employée comme liquide d’essai, le rapport d’essai doit indiquer la masse volumique, l’indice de réfraction, la viscosité et le point d’aniline ou la teneur en aromatiques de l’huile. Les huiles utilisées en service qui présentent des caractéristiques de fluides analogues aux liquides de référence (voir Article A.1 à Article A.3) n’auront pas nécessairement le même effet sur le matériau que ces derniers. Certains carburants, en particulier l’essence, varient largement de composition et dans le cas de certains constituants, des variations minimes peuvent avoir une grande influence sur l’effet exercé sur le caoutchouc. Tous les détails de la composition du carburant utilisé doivent donc être inclus dans le rapport d’essai.

Les fluides de travail des métaux (MWF) ou les lubrifiants réfrigérants sont utilisés dans les ateliers du monde entier pour la coupe et le formage des métaux. Ils servent principalement à refroidir et à lubrifier les outils, les pièces à usiner et les machines, à inhiber la corrosion et à éliminer les copeaux. Les MWF sont disponibles sous forme d'huiles non hydrosolubles, de concentrés hydrosolubles ou émulsifiables ou de produits entièrement synthétiques sans huile. Les MWF non hydrosolubles sont principalement constitués d'une huile de base (généralement à plus de 95 %). Il peut s'agir d'une huile minérale, d'une huile d’ester (par exemple l'huile de colza non raffinée ou modifiée chimiquement) ou d'une huile synthétique (par exemple la poly-alpha-oléfine). Pour les essais, elles peuvent être utilisées telles qu'elles sont expédiées. Les MWF hydrosolubles sont mélangés à de l'eau avant utilisation, à des concentrations de 2 % à 25 %, en fonction du produit et du type d'usinage. Ce type de MWF est à base d'huile et des proportions de 20 % à 80 % sont possibles. Pour combiner cette huile avec l'eau et obtenir une émulsion huile dans l'eau, un émulsifiant est nécessaire. Les fluides entièrement ou semi-synthétiques sont hydrosolubles et ne nécessitent pas d'émulsifiants. Ils peuvent être à base de composés de glycol hydrosolubles, par exemple. Le mélange dans l'eau donne un MWF transparent. Les essais de compatibilité des joints peuvent être réalisés soit avec le concentré fourni, soit avec une émulsion ou solution fraîchement préparée. Pour mélanger une émulsion ou solution d'essai, il convient d'utiliser de l'eau désionisée à température ambiante. La concentration standard est une fraction massique de 10 %, mais d'autres concentrations peuvent être utilisées si nécessaire. Il convient que le fluide pour travail des métaux concentré soit ajouté lentement à l'eau avec agitation (par exemple à l'aide d'un agitateur magnétique), afin d'éviter la gélification ou le fractionnement de l'émulsion. Étant donné que les liquides commerciaux peuvent ne pas avoir une composition tout à fait constante, un liquide normalisé constitué de composés chimiques ou de mélanges de composés chimiques bien définis, conformément à l’Annexe A, doit être utilisé comme liquide de référence aux fins de la classification des caoutchoucs vulcanisés ou du contrôle de qualité.

Lors des essais destinés à déterminer l’effet des solutions chimiques, la concentration des solutions doit être adaptée à l’application envisagée.

Selon la température, la composition du liquide d’essai peut varier de manière significative au cours de l’immersion. Le vieillissement du liquide d’essai et toute interaction avec les éprouvettes doivent être pris en considération. Si le liquide contient des additifs chimiquement actifs ou si une variation significative de la composition est observée par extraction, absorption ou réaction du caoutchouc, soit le volume doit être

ISO 1817:2026(fr) augmenté soit le liquide doit être remplacé par un nouveau liquide à des intervalles spécifiés. Voir 9.2 pour plus d’informations.

Certains liquides sont sensibles à l'oxydation. Ainsi, ils peuvent subir des modifications importantes lorsqu'ils sont exposés à l'air à une température élevée, ce qui peut être le cas dans la Méthode C. NOTE Il a été démontré que lors de l'utilisation d'huiles commerciales contenant des additifs, il n'est pas uniquement important d'empêcher l'entrée d'air, mais aussi l'échappement de produits volatils du récipient d'immersion (les produits de dégradation de l'huile ou de ses additifs peuvent être très agressifs).

7 Éprouvettes

7.1 Préparation

Les éprouvettes doivent être préparées conformément à l’ISO 23529.

7.2 Dimensions

Les données obtenues avec des éprouvettes présentant différentes épaisseurs initiales ne sont pas toujours comparables. Par conséquent, les éprouvettes doivent, dans la mesure du possible, avoir une épaisseur uniforme de (2 ± 0,2) mm.

Des éprouvettes découpées dans des produits finis peuvent être utilisées. Pour des produits finis d’épaisseur inférieure à 1,8 mm, utiliser l’épaisseur initiale. Pour des produits d’épaisseur supérieure à 2,2 mm, réduire l’épaisseur à (2 ± 0,2) mm (voir ISO 23529).

Les éprouvettes utilisées pour la détermination de la variation de volume et de masse doivent avoir un 3 3 volume de 1 cm à 3 cm .

Les éprouvettes utilisées pour la détermination de la variation de dureté doivent avoir des dimensions latérales au moins égales à 8 mm.

...