ISO 8006:1985
(Main)Carbonaceous materials used in the production of aluminium — Pitch for electrodes — Determination of ash
Carbonaceous materials used in the production of aluminium — Pitch for electrodes — Determination of ash
A test portion is deated in a tared platinum crucible, in a furnace at 700 degrees centigrade, under oxidizing and specified conditions, to constant mass. The residue is cooles and weighed. The method is applicable to products (tar pitch, petroleum pitch, etc.) producing a quality of ash greater than or equal to 0,05 % (m/m).
Produits carbonés utilisés pour la production de l'aluminium — Brai pour électrodes — Détermination du taux de cendres
La présente Norme internationale spécifie une méthode de détermination du taux de cendres des brais pour électrodes utilisés pour la production de l'aluminium. La méthode est applicable aux produits (brai de goudron, de pétrole, etc.) dont le taux de cendres est supérieur ou égal à 0,05 % (m/m) sur les produits tels quels. S'il est demandé d'exprimer le résultat par rapport au produit sec, déterminer la teneur en eau du produit par entraînement azéotropique selon la méthode spécifiée dans l'ISO 5939 et, à partir du résultat de la détermination des cendres obtenu sur le produit tel quel, en déduire le taux de cendres pour le produit sec. NOTE -- Les cendres peuvent être utilisées pour le dosage ultérieur des éléments.
General Information
- Status
- Published
- Publication Date
- 28-Aug-1985
- Technical Committee
- ISO/TC 226 - Materials for the production of primary aluminium
- Drafting Committee
- ISO/TC 226 - Materials for the production of primary aluminium
- Current Stage
- 9093 - International Standard confirmed
- Start Date
- 27-Oct-2025
- Completion Date
- 12-Feb-2026
Overview
ISO 8006:1985 applies to carbonaceous materials used in aluminium production - specifically pitch for electrodes (tar pitch, petroleum pitch, etc.) - and specifies a gravimetric method for the determination of ash. The method is intended for products that yield an ash content greater than or equal to 0.05 % (m/m). The procedure uses a tared platinum crucible and controlled oxidizing incineration in a furnace at 700 ± 10 °C until constant mass is achieved.
Key Topics
Scope and applicability: Designed for electrode pitch materials in the aluminium industry with ash ≥ 0.05 % (m/m).
Apparatus:
- Platinum crucible (low form), capacity ~50 ml.
- Electric furnace adjustable up to 700 ± 10 °C with air circulation.
- Drying oven adjustable to 150 ± 5 °C and desiccator with P2O5.
- Analytical balance with precision to 0.0002 g for weighing crucible and residues.
Sampling and preparatory tests: Sampling is to follow ISO 6257; if results must be reported on a dry basis, determine moisture according to ISO 5939 (Dean and Stark azeotropic method).
Procedure summary:
- Preheat/crucible conditioning (e.g., 1 h at 700 ± 10 °C) and cooling in desiccator.
- Weigh crucible (m1) to 0.0002 g precision, add ~5 g test portion (mo) and place in furnace.
- Heat in stages (e.g., starting ≈300 ± 10 °C, then 350, 400, 450 °C with controlled ramping and holds of not less than 30 min - to avoid rapid volatilization) before final heating at 700 ± 10 °C until incineration is complete and constant mass is reached.
- Cool first to ~100–150 °C in air, then to ambient in a desiccator with P2O5 and weigh (m2).
Calculation: Express ash on the as‑received sample as percentage by mass to 0.01 % (m/m) using the equation:
x = ((m2 - m1) / mo) × 100
where m1 = mass of empty crucible, m2 = mass of crucible + ash residue, mo = mass of test portion.
Performance: Precision (repeatability and reproducibility) is addressed per ISO 5725; graphical and statistical correlation between repeatability and reproducibility are reported in the standard.
Applications
- Quality control of electrode pitch suppliers and incoming raw materials for aluminium smelting operations.
- Material certification and batch release testing to confirm ash limits and compliance with procurement specifications.
- Useful for laboratories conducting routine ash determinations as part of process control, acceptance testing, or comparative material assessment.
Related Standards
- ISO 6257 - Sampling of pitch for electrodes (referenced for correct sample selection).
- ISO 5939 - Determination of water in carbonaceous products (Dean and Stark azeotropic method) for dry-basis reporting.
- ISO 5725 - Precision of test methods (repeatability and reproducibility) for interlaboratory performance assessment.
ISO 8006:1985 is a practical, standardized gravimetric procedure that supports reproducible ash determination and helps maintain consistent quality in carbonaceous materials used for electrode manufacture in the aluminium industry.
ISO 8006:1985 - Carbonaceous materials used in the production of aluminium -- Pitch for electrodes -- Determination of ash
ISO 8006:1985 - Produits carbonés utilisés pour la production de l'aluminium -- Brai pour électrodes -- Détermination du taux de cendres
ISO 8006:1985 - Produits carbonés utilisés pour la production de l'aluminium -- Brai pour électrodes -- Détermination du taux de cendres
Get Certified
Connect with accredited certification bodies for this standard

ECOCERT
Organic and sustainability certification.

Eurofins Food Testing Global
Global leader in food, environment, and pharmaceutical product testing.

Intertek Bangladesh
Intertek certification and testing services in Bangladesh.
Sponsored listings
Frequently Asked Questions
ISO 8006:1985 is a standard published by the International Organization for Standardization (ISO). Its full title is "Carbonaceous materials used in the production of aluminium — Pitch for electrodes — Determination of ash". This standard covers: A test portion is deated in a tared platinum crucible, in a furnace at 700 degrees centigrade, under oxidizing and specified conditions, to constant mass. The residue is cooles and weighed. The method is applicable to products (tar pitch, petroleum pitch, etc.) producing a quality of ash greater than or equal to 0,05 % (m/m).
A test portion is deated in a tared platinum crucible, in a furnace at 700 degrees centigrade, under oxidizing and specified conditions, to constant mass. The residue is cooles and weighed. The method is applicable to products (tar pitch, petroleum pitch, etc.) producing a quality of ash greater than or equal to 0,05 % (m/m).
ISO 8006:1985 is classified under the following ICS (International Classification for Standards) categories: 71.100.10 - Materials for aluminium production. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO 8006:1985 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
International Standard
INTERNATIONAL ORGANIZATION FOR STANDARDlZATION.MEX~YHAPO~HAR OPrAHM3ALWlR I-IO CTAH~APTM3AlJMM.ORGANISATlON INTERNATIONALE DE NORMALISATION
Carbonaceous materials used in the production
of aluminium - Pitch for electrodes -
Determination of ash
Produits carbonhs utilisks pour Ia production de l’aluminium - Brai pour t!lectrodes - Determination du taux de cendres
First edition - 1985-09-01
UDC 665.777 : 669.713 : 543.822 kef. No. ISO 80064985 (E)
eiectrodes, pitch (material& tests, ash determination.
Descriptors : aluminium, production, industrial products,
Price based on 3 pages
Foreword
ISO (the International Organization for Standardization) is a worldwide federation of
national Standards bodies (ISO member bodies). The work of preparing International
Standards is normally carried out through ISO technical committees. Esch member
body interested in a subject for which a technical committee has been established has
the right to be represented on that committee. International organizations, govern-
mental and non-governmental, in liaison with ISO, also take part in the work.
Draft International Standards adopted by the technical committees are circulated to
the member bodies for approval before their acceptance as International Standards by
the ISO Council. They are approved in accordance with ISO procedures requiring at
least 75 % approval by the member bodies voting.
International Standard ISO 8006 was prepared by Technical Committee ISO/TC 47,
Cbemistry.
International Organkation for Standardkation, 1985
Printed in Switzerland
ISO 8006-1985 (E)
INTERNATIONAL STANDARD
Carbonaceous materials used in the production
Pitch for electrodes -
of aluminium -
Determination of ash
1 Scope and field of application 5 Sampling and samples
This International Standard specifies a method for the deter- Sample in accordance with ISO 6257.
mination of ash in the pitch for electrodes used in the produc-
tion of aluminium.
6 Procedure
The method is applicable to products (tar pitch, Petroleum
pitch, etc.) producing a quantity of ash greater than or equal to
6.1 Test Portion
0,05 % (mlm).
Heat the crucible (4.1) for 1 h in the furnace (4.21, controlled at
If it is required to express the result on the dry product, carry
700 + - 10 OC. Allow the crucible to cool, first in air to about 100
out the water determination by azeotropic distillation as
and 150 OC, and then in a desiccator charged with diphos-
specified in ISO 5939. Refer the result of the determination of
phorus pentaoxide, to room temperature. Weigh the crucible to
ash obtained on the product as such, to the dry product.
the nearest 0,000 2 g (m,).
NOTE - This ash may be utilised for subsequent elemental analysis.
Weigh into the crucible, to the nearest 0,000 2 g, approxi-
mately 5 g of the test Sample (sec clause 5) (mol.
2 Refarences
6.2 Determination
ISO 5725, Precision of test methods - Determination of
repeatability and reproducibility b y inter-laboratory tests.
Place the crucible containing the test Portion (6.1) into the
electric furnace (4.2) set at a temperature close to but not ex-
ISO 5939, Carbonaceous materials for the production of
ceeding 300 + 10 OC. Increase heating following the heating
aluminium. Determination o f water con ten t - Azeo tropic
rule indicated below.
distrllation fDean and Stark).
In periods of not less than 30 min each, but which may,
ISO 6257, Carbonaceous materials for the production of
without prejudice, be increased to approximately 60 min, raise
aluminium - Pitch for electrodes - Sampling.
the temperature at a uniform rate first to 350 + 10 OC, then to
400 I!I 10 OC and finally to 450 31 10 OC, inspecting regularly
to ensure that no mechanical loss of the test Portion occurs due
3 Principle
to over-vigorous volatilization. lf losses are observed, repeat
the determination on another test portion and following the
Heating of a test Portion in a tared platinum crucible, in a fur-
procedure specified below.
nace at 700 OC, under oxi
...
Norme internationale @ 8006
INTERNATIONAL ORGANIZATION FOR STANDARDIZATION*MEXLYHAPOLHAR OPTAHHJAUHR Il0 CTAHAAPTH3A~HM*ORGANlSATlON INTERNATIONALE DE NORMALISATION
Produits carbonés utilisés pour la production de
l'aluminium - Brai pour électrodes - Détermination du
taux de cendres
Carbonaceous materials used in the production of aluminium - Pitch for electrodes - Determination of ash
Premiere 6dition - 1985-09-01
- iî CDU 665.777 : 669.713 : 543.822 R6f. no : IS0 8006-1985 (FI
Descripteurs : aluminium, production, produit industriel, Blectrode, brai, essai, dosage des cendres.
3 pages
Prix bas6 sur
Ava n t- p r op os
L‘ISO (Organisation internationale de normalisation) est une federation mondiale
d‘organismes nationaux de normalisation (cornites membres de I‘ISO). L’blaboration
des Normes internationales est confiée aux cornites techniques de I’ISO. Chaque
cornite membre intéresse par une étude a le droit de faire partie du cornite technique
crée B cet effet. Les organisations internationales, gouvernementales et non gouverne-
mentales, en liaison avec I’ISO, participent Bgalement aux travaux.
Les projets de Normes internationales adoptes par les cornites techniques sont soumis
aux cornites membres pour approbation, avant leur acceptation comme Normes inter-
I’ISO. Les Normes internationales sont approuvees confor-
nationales par le Conseil de
mement aux procedures de I‘ISO qui requihrent l’approbation de 75 % au moins des
cornites membres votants.
La Norme internationale IS0 8006 a et6 Blaboree par le cornite technique ISO/TC 47,
Chimie.
O Organisation internationale de normalisation, 1985 0
Imprimé en Suisse
IS0 8006-1985 (F)
NORM E I NTE R NAT1 ON ALE
Produits carbonés utilisés pour la production de
l'aluminium - Brai pour électrodes - Détermination du
taux de cendres
1 Objet et domaine d'application
5 Échantillonnage et échantillons
La présente Norme internationale spécifie une méthode de
Échantillonner suivant I'ISO 6257.
détermination du taux de cendres des brais pour électrodes uti-
lisés pour la production de l'aluminium.
6 Mode operatoire
La méthode est applicable aux produits (brai de goudron, de
pétrole, etc.) dont le taux de cendres est supérieur ou égal à
6.1 Prise d'essai
0,05 % (m/m) sur les produits tels quels.
Chauffer le creuset (4.1) durant 1 h dans le four (4.2) réglé à
S'il est demande d'exprimer le resultat par rapport au produit
700 k 10 OC. Laisser refroidir le creuset d'abord à l'air entre
sec, determiner la teneur en eau du produit par entraînement
100 et 150 OC environ, puis dans un dessiccateur garni de
azeotropique selon la méthode specifiée dans I'ISO 5939 et, à
pentaoxyde de diphosphore jusqu'à la température ambiante.
partir du resultat de la determination des cendres obtenu sur le
Peser le creuset à 0,OOO 2 g près (m,).
produit tel quel, en déduire le taux de cendres pour le produit sec.
Peser, à 0,ooO 2 g près, dans le creuset ainsi taré, 5 g environ
NOTE - Les cendres peuvent &re utilisees pour le dosage ulterieur des
de I'échantillon pour essai (voir chapitre 5) (mo).
BIBments.
6.2 D6terrnination
2 Références
Placer le creuset contenant la prise d'essai (6.1) dans le four
IS0 5725, Fidelite des methodes d'essai - Determination de la électrique (4.2) réglé à une température voisine mais non supé-
rep6tabilit.4 et de la reproductibilitB par essais interlaboratoires. rieure à 300 ? 10 OC. Augmenter le chauffage en suivant la
règle indiquée ci-après.
IS0 5939, Produits carbones utilisBs pour la production de
l'aluminium - Brai pour 6lectrodes - Dosage de l'eau - Dans des périodes de temps non inferieures à 30 min, mais qui
Methode par entraînement azdotropique YDean et Stark). peuvent être prolongées même jusqu'à 60 min environ sans
inconvénient, élever la température de manière uniforme à
IS0 6257, Produits carbones utilisBs pour la production de 350 ? 10 OC puis à 400 k 10 OC et finalement A 450 f 10 OC,
en contralant à intervalles réguliers pour s'assurer qu'il n'y a
l'aluminium - Brai pour Blectrodes - Échantillonnage.
pas de pertes mécaniques de prise d'essai provoquées par une
volatilisation trop rapide. Si l'on observe de telles pertes, répé-
ter l'opération sur une autre prise d'essai selon les modalites
3 Principe
spécifiées
...
Norme internationale
INTERNATIONAL ORGANIZATION FOR STANDARDIZATIONWIE~YHAPO~HAR OPI-AHH3AlWlR fl0 CTAH~APTbI3AlWl~RGANISATION INTERNATIONALE DE NORMALISATION
Produits carbonés utilisés pour la production de
- Brai pour électrodes - Détermination du
l’aluminium
taux de cendres
Carbonaceous materials used in the production of aluminium - Pitch for electrodes - Determination of ash
Première édition - 198549-01
~~ -~~
Réf. no : ISO 8006-1985 (F)
CDU 665.777 : 669.713 : 543.822
aluminium, production, produit industriel, électrode, brai, essai, dosage des cendres.
Descripteurs :
Prix basé sur 3 pages
Avant-propos
LYS0 (Organisation internationale de normalisation) est une fédération mondiale
d’organismes nationaux de normalisation (comités membres de I’ISO). L’élaboration
des Normes internationales est confiée aux comités techniques de I’ISO. Chaque
comité membre intéresse par une étude a le droit de faire partie du comité technique
créé à cet effet. Les organisations internationales, gouvernementales et non gouverne-
mentales, en liaison avec I’ISO, participent également aux travaux.
Les projets de Normes internationales adoptés par les comités techniques sont soumis
aux comités membres pour approbation, avant leur acceptation comme Normes inter-
nationales par le Conseil de I’ISO. Les Normes internationales sont approuvées confor-
mément aux procédures de I’ISO qui requièrent l’approbation de 75 % au moins des
comités membres votants.
La Norme internationale ISO 8006 a été élaborée par le comite technique ISO/TC 47,
Chimie.
0 Organisation internationale de normalisation, 1985
Imprimé en Suisse
ISO 80064985 (F)
NORME INTERNATIONALE
Produits carbonés utilisés pour la production de
- Brai pour électrodes - Détermination du
l’aluminium
taux de cendres
1 Objet et domaine d’application 5 Échantillonnage et échantillons
La présente Norme internationale spécifie une méthode de Échantillonner suivant I’ISO 6257.
détermination du taux de cendres des brais pour électrodes uti-
lisés pour la production de l’aluminium.
6 Mode opératoire
La méthode est applicable aux produits (brai de goudron, de
pétrole, etc.) dont le taux de cendres est supérieur ou égal à
6.1 Prise d’essai
0,05 % (mlm) sur les produits tels quels.
Chauffer le creuset (4.1) durant 1 h dans le four (4.2) réglé à
S’il est demandé d’exprimer le résultat par rapport au produit
700 + 10 OC. Laisser refroidir le creuset d’abord à l’air entre
sec, déterminer la teneur en eau du produit par entraînement
100 et 150 OC environ, puis dans un dessiccateur garni de
azéotropique selon la méthode spécifiée dans I’ISO 5939 et, à
pentaoxyde de diphosphore jusqu’à la température ambiante.
partir du résultat de la détermination des cendres obtenu sur le
Peser le creuset à 0,000 2 g près (ml).
produit tel quel, en déduire le taux de cendres pour le produit sec.
Peser, à 0,006 2 g prés, dans le creuset ainsi taré, 5 g environ
NOTE - Les cendres peuvent être utilisées pour le dosage ultérieur des
de l’échantillon pour essai (voir chapitre 5) (m&
éléments.
6.2 Détermination
2 Références
Placer le creuset contenant la prise d’essai (6.1) dans le four
électrique (4.2) réglé à une température voisine mais non supé-
ISO 5725, Fidelite des methodes d’essai - Determination de la
répétabilité et de la reproductibilite par essais interlaboratoires. rieure à 300 + 10 OC. Augmenter le chauffage en suivant la
règle indiquée ci-après.
ISO 5939, Produits carbones utilises pour la production de
l’aluminium - Brai pour electrodes - Dosage de l’eau - Dans des périodes de temps non inférieures à 30 min, mais qui
Methode par entraînement azeotropigue -(Dean et Stark). peuvent être prolongées même jusqu’à 60 min environ sans
inconvénient, élever la température de manière uniforme à
ISO 6257, Produits carbones utilises pour la production de 350 + 10 OC puis à 400 + 10 OC et finalement a450 + 10 OC,
en contrôlant à intervalles réguliers pour s’assurer qu’il n’y a
l’aluminium - Brai pour elec trodes - Échantillonnage.
pas de pertes mécaniques de prise d’essai provoquées par une
volatilisation
...












Questions, Comments and Discussion
Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.
Loading comments...