Standard Test Method for Quinoline-Insoluble (QI) Content of Tar and Pitch

SIGNIFICANCE AND USE
4.1 This test method is useful in evaluating and characterizing tar and pitch, and as one element in establishing the uniformity of shipments and sources of supply.
SCOPE
1.1 This test method covers the determination of the quinoline-insoluble matter (QI) in tar and pitch.  
1.2 Since this test method is empirical, strict adherence to all details of the procedure is necessary.  
1.3 The values stated in SI units are to be regarded as standard. No other units of measurement are included in this standard.  
1.4 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use. For hazards information, see Section 7.

General Information

Status
Historical
Publication Date
30-Nov-2015
Current Stage
Ref Project

Relations

Buy Standard

Standard
ASTM D2318-15 - Standard Test Method for Quinoline-Insoluble (QI) Content of Tar and Pitch
English language
4 pages
sale 15% off
Preview
sale 15% off
Preview
Standard
REDLINE ASTM D2318-15 - Standard Test Method for Quinoline-Insoluble (QI) Content of Tar and Pitch
English language
4 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D2318 − 15
Standard Test Method for
1
Quinoline-Insoluble (QI) Content of Tar and Pitch
This standard is issued under the fixed designation D2318; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope* 3. Summary of Test Method
1.1 This test method covers the determination of the 3.1 The sample is digested in hot quinoline and filtered.The
quinoline-insoluble matter (QI) in tar and pitch. insoluble material is washed, dried, and weighed.
1.2 Since this test method is empirical, strict adherence to
4. Significance and Use
all details of the procedure is necessary.
4.1 This test method is useful in evaluating and character-
1.3 The values stated in SI units are to be regarded as
izing tar and pitch, and as one element in establishing the
standard. No other units of measurement are included in this
uniformity of shipments and sources of supply.
standard.
1.4 This standard does not purport to address all of the
5. Apparatus
safety concerns, if any, associated with its use. It is the
5.1 Filtering Crucibles, porcelain, with fine-porosity
responsibility of the user of this standard to establish appro-
bottom, 25 mL to 40 mL capacity, high-form, maximum pore
priate safety and health practices and determine the applica-
diameter, 7 µm.
bility of regulatory limitations prior to use. For hazards
information, see Section 7. 5.2 Filter Apparatus—Filter flask and tube with crucible
adapter.
2. Referenced Documents
5.3 Sieves—U. S. Standard 600 µm (No. 30) and 250 µm
2
2.1 ASTM Standards:
(No. 60), conforming to Specification E11.
D71 Test Method for Relative Density of Solid Pitch and
5.4 Electric Hot Plate or Water Bath,maintainedat75 °C 6
Asphalt (Displacement Method)
5 °C.
D95 Test Method for Water in Petroleum Products and
Bituminous Materials by Distillation
6. Reagents and Materials
D329 Specification for Acetone
D362 SpecificationforIndustrialGradeToluene(Withdrawn 6.1 Quinoline, Refined,meetingthefollowingrequirements:
3
1989) 6.1.1 The quinoline shall distill from 5 % to 95 % within a
D850 Test Method for Distillation of Industrial Aromatic range of 2 °C that shall include the temperature of 237.4 °C
Hydrocarbons and Related Materials after corrections for barometric pressure and emergent stem
D4296 Practice for Sampling Pitch have been applied. The distillation shall be carried out in
D7280 Test Method for Quinoline-Insoluble (QI) Content of accordance with Test Method D850 using a total immersion
Tar and Pitch by Stainless Steel Crucible Filtration thermometer with a range from 195 °C to 305 °C, graduated in
E1 Specification for ASTM Liquid-in-Glass Thermometers 0.5 °C, and conforming to the requirements for Thermometer
E11 Specification for Woven Wire Test Sieve Cloth and Test 69C as described in Specification E1. Temperature measuring
Sieves devices such as precision thermocouples, resistance tempera-
ture detectors (RTDs), and liquid-in-glass thermometers with
equal or better accuracies in the appropriate temperature range
1
This test method is under the jurisdiction of ASTM Committee D02 on
may be used.
Petroleum Products, Liquid Fuels, and Lubricantsand is the direct responsibility of
SubcommitteeD02.05onPropertiesofFuels,PetroleumCokeandCarbonMaterial.
6.1.2 The quinoline shall have a specific gravity at 15.5/
Current edition approved Dec. 1, 2015. Published December 2015. Originally
15.5 °C of 1.092 to 1.098, as determined by Test Method D71,
ɛ1
approved in 1964. Last previous edition approved in 2014 as D2318 – 14 . DOI:
or other method of equivalent accuracy.
10.1520/D2318-15.
2
6.1.3 Thequinolineshallbeclearandlightincolorandshall
For referenced ASTM standards, visit the ASTM website, www.astm.org, or
contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM
contain less than 0.5 % volume of water as determined byTest
Standards volume information, refer to the standard’s Document Summary page on
Method D95. If not, redistill the quinoline in all-glass
the ASTM website.
3
apparatus, discarding the first 5 % and collecting the next
The last approved version of this historical standard is referenced on
www.astm.org. 90 %. If the quinoline contains suspended matter but is clear,
*A Summary of Changes section appears at the end of this standard
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
D2318 − 15
light in color, and contains less than 0.5 % water, filter the 10. Preparation of Working Sample
quinolinethroughacruciblecontaining5gofCeliteFilterAid
...

This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
´1
Designation: D2318 − 14 D2318 − 15
Standard Test Method for
1
Quinoline-Insoluble (QI) Content of Tar and Pitch
This standard is issued under the fixed designation D2318; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1
ε NOTE—Editorial changes were made throughout the test method in September 2014.
1. Scope*
1.1 This test method covers the determination of the quinoline-insoluble matter (QI) in tar and pitch.
1.2 Since this test method is empirical, strict adherence to all details of the procedure is necessary.
1.3 The values stated in SI units are to be regarded as standard. No other units of measurement are included in this standard.
1.4 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility
of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory
limitations prior to use. For hazards information, see Section 7.
2. Referenced Documents
2
2.1 ASTM Standards:
D71 Test Method for Relative Density of Solid Pitch and Asphalt (Displacement Method)
D95 Test Method for Water in Petroleum Products and Bituminous Materials by Distillation
D329 Specification for Acetone
3
D362 Specification for Industrial Grade Toluene (Withdrawn 1989)
D850 Test Method for Distillation of Industrial Aromatic Hydrocarbons and Related Materials
D4296 Practice for Sampling Pitch
D7280 Test Method for Quinoline-Insoluble (QI) Content of Tar and Pitch by Stainless Steel Crucible Filtration
E1 Specification for ASTM Liquid-in-Glass Thermometers
E11 Specification for Woven Wire Test Sieve Cloth and Test Sieves
3. Summary of Test Method
3.1 The sample is digested in hot quinoline and filtered. The insoluble material is washed, dried, and weighed.
4. Significance and Use
4.1 This test method is useful in evaluating and characterizing tar and pitch, and as one element in establishing the uniformity
of shipments and sources of supply.
5. Apparatus
5.1 Filtering Crucibles, porcelain, with fine-porosity bottom, 25 mL to 40 mL capacity, high-form, maximum pore diameter, 7
μm.
5.2 Filter Apparatus—Filter flask and tube with crucible adapter.
5.3 Sieves—U. S. Standard 600 μm (No. 30) and 250 μm (No. 60), conforming to Specification E11.
5.4 Electric Hot Plate or Water Bath, maintained at 75 °C 6 5 °C.
1
This test method is under the jurisdiction of ASTM Committee D02 on Petroleum Products, Liquid Fuels, and Lubricantsand is the direct responsibility of Subcommittee
D02.05 on Properties of Fuels, Petroleum Coke and Carbon Material.
Current edition approved May 1, 2014Dec. 1, 2015. Published May 2014December 2015. Originally approved in 1964. Last previous edition approved in 20132014 as
ɛ1
D2318 – 98 (2013).D2318 – 14 . DOI: 10.1520/D2318-14E01.10.1520/D2318-15.
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards
volume information, refer to the standard’s Document Summary page on the ASTM website.
3
The last approved version of this historical standard is referenced on www.astm.org.
*A Summary of Changes section appears at the end of this standard
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
D2318 − 15
6. Reagents and Materials
6.1 Quinoline, Refined, meeting the following requirements:
6.1.1 The quinoline shall distill from 5 % to 95 % within a range of 2 °C that shall include the temperature of 237.4 °C after
corrections for barometric pressure and emergent stem have been applied. The distillation shall be carried out in accordance with
Test Method D850 using a total immersion thermometer with a range from 195 °C to 305 °C, graduated in 0.5 °C, and conforming
to the requirements for Thermometer 69C as described in Specification E1. Temperature measuring devices such as precision
thermocouples, resistance temperature detectors (RTDs), and liquid-in-glass thermometers with equal or better accuracies in the
appropriate temperature range may be used.
6.1.2 The quinoline shall have a specific gravity at 15.5/15.5 °C of 1.092 to 1.098, as determined by Test Method D71, or other
method of equivalent acc
...

Questions, Comments and Discussion

Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.