EN ISO 17947-1:2026
(Main)Fine ceramics (advanced ceramics, advanced technical ceramics) - Methods for chemical analysis of silicon nitride powders - Part 1: Wet chemical methods, X-ray fluorescence (XRF) using the fused cast-bead method, carrier-gas hot extraction (CGHE) and combustion methods (ISO 17947-1:2026)
- Abstract
This document specifies methods for the determination of silicon, nitrogen, aluminium, iron, calcium, oxygen, carbon, fluorine, and chlorine in silicon nitride powders.
This document is applicable for the chemical analysis of silicon nitride powders used as raw material for fine ceramics.
- Status
- Published
- Publication Date
- 03-Nov-2026
- Technical Committee
- CEN/TC 184 - Advanced technical ceramics
- Current Stage
- 6060 - Definitive text made available (DAV) - Publishing
- Start Date
- 04-Nov-2026
- Due Date
- 04-Nov-2026
- Completion Date
- 04-Nov-2026
EN ISO 17947-1:2026 is a CEN standard for chemical analysis of silicon nitride powders used as raw material for fine ceramics. It specifies methods for determining silicon, nitrogen, aluminium, iron, calcium, oxygen, carbon, fluorine, and chlorine, so laboratories can choose a suitable method and report results on the dried sample.
What does EN ISO 17947-1:2026 specify?
EN ISO 17947-1:2026 applies to silicon nitride powders used as raw material for fine ceramics. It sets out how to determine the listed major, minor and trace constituents by wet chemical methods, X-ray fluorescence (XRF) using the fused cast-bead method, carrier-gas hot extraction (CGHE), and combustion methods.
The document is organized into clauses 1 to 14. The early clauses cover scope, normative references, analyte ranges, sample preparation, apparatus and reagents, and blank tests. Later clauses give the element-by-element methods, reporting rules, and the test report.
| Annex | What it covers |
|---|---|
| Annex A | Commercial certified reference materials |
| Annex B | Round robin test results |
| Annex C | Spectral lines for ICP-OES |
What are the key requirements of EN ISO 17947-1:2026?
Clause 3 sets the analyte ranges. EN ISO 17947-1:2026 gives ranges for silicon, nitrogen, aluminium, iron, calcium, oxygen, carbon, fluorine, and chlorine. In practice, this tells the user whether the standard method is suited to the material and whether the expected result sits in the intended working range.
Clause 4 controls sampling, drying and weighing. Sampling follows ISO 8656-1 unless the analyser and customer agree otherwise, and the test sample is dried before analysis. The sample is weighed to the nearest 0.1 mg, which matters because the final result is reported as a mass fraction on the dried sample.
Clause 6 requires a blank test for each determination. The blank uses the same reagents, conditions and procedure as the sample run. This matters because it corrects for reagent background and contamination, which can be important at low analyte levels.
Clause 7 gives two silicon routes. EN ISO 17947-1:2026 allows method A, fusion-dehydration/insolubilization separation with gravimetry and inductively coupled plasma optical emission spectrometry (ICP-OES), or method B, XRF using the fused cast-bead method. Method A is for results with four figures, while method B can be used when two or three figures are enough, so the user can match precision to the reporting need and available equipment.
Clause 8 gives three nitrogen routes. The standard provides acid pressure decomposition-distillation separation-acidimetric titration, inert gas fusion-thermal conductivity, and fusion-ammonia separation-acidimetric titration. Method A includes a recovery check using ammonium sulfate, and method B requires calibration with a nitride whose oxygen content is close to the sample, which helps avoid bias from matrix differences.
Clauses 9 and 10 cover aluminium, iron, calcium, and oxygen by ICP-OES or gas analysis. Aluminium, iron and calcium are measured after pressure decomposition and silicon removal, then calibrated against matrix-matched solutions. Oxygen is measured by inert gas fusion with an infrared (IR) detector, with calibration using yttrium oxide or a nitride with known oxygen content. In practice, these clauses show how to separate the element from the ceramic matrix before measuring it.
Clauses 11 and 12 cover carbon, fluorine and chlorine. Carbon can be determined by combustion with IR absorption spectrometry, coulometry, or thermal conductivity, while fluorine and chlorine are extracted by pyrohydrolysis and then measured by ion chromatography or spectrophotometry. This matters because the document supports both simultaneous and separate measurement routes depending on the laboratory setup.
Clause 13 sets the reporting rule. Each sample is analysed twice on different days, and the result is accepted by comparison with the tolerances in Table 1. If the two values are outside tolerance, two more analyses are made and the median of four values may be reported. Results are expressed as mass fractions in percent, with two decimal places for silicon and nitrogen and three for the other analytes.
What terms does EN ISO 17947-1:2026 define?
- Blank test - A run made with the same reagents and procedure as the sample, used to correct the final result for background contamination.
- Mass fraction - The amount of an element reported as a percentage of the dried sample.
- Calibration coefficient - The factor used to convert an instrument reading into content for oxygen, nitrogen or carbon methods.
- XRF - X-ray fluorescence, used here with the fused cast-bead method for silicon.
- CGHE - Carrier-gas hot extraction, a gas-analysis route used in the document for elemental determination.
- ICP-OES - Inductively coupled plasma optical emission spectrometry, used for silicon in method A and for aluminium, iron and calcium.
- Pyrohydrolysis - Heating the sample in steam and oxygen to release fluorine and chlorine for measurement.
Who uses EN ISO 17947-1:2026?
EN ISO 17947-1:2026 is used by analytical laboratories, fine ceramics producers, raw material suppliers, quality control teams and buyers who need verified composition data for silicon nitride powder. It is relevant for incoming inspection, process control, certificate checking and supplier qualification. It also supports laboratories that need a documented way to compare results across different methods and instruments.
What changed in EN ISO 17947-1:2026 from the previous edition?
EN ISO 17947-1:2026 was developed from JIS R 1603:2007, with reference to CEN ENV 14226:2002 and ASTM C1494-01:2007. The document also states that it applies to silicon nitride raw powders for fine ceramics use.
Which standards are used with EN ISO 17947-1:2026?
- ISO 2828 - Used for the spectrophotometric fluorine route.
- ISO 3696 - Specifies the water quality for analytical use.
- ISO 6353-1, ISO 6353-2 and ISO 6353-3 - Give reagent test methods and specifications.
- ISO 8656-1 - Provides the sampling scheme for raw materials and unshaped products.
- ISO 21068-2 - Supplies alternative procedures used for silicon, nitrogen and carbon in several clauses.
- ISO 21068-3 - Supplies alternative procedures for XRF and for nitrogen by fusion-ammonia separation.
- ISO 21438-2 and ISO 21438-3 - Support the ion chromatography routes for chlorine and fluorine.
- ISO 26845 - Gives general requirements for wet chemical analysis and related instrumental methods.
What does the EN ISO 17947-1:2026 document contain?
The document contains the analyte ranges, sample preparation instructions, apparatus and reagent requirements, blank-test rules, and detailed procedures for silicon, nitrogen, aluminium, iron, calcium, oxygen, carbon, fluorine and chlorine. It also includes calculation formulae for each analytical route, reporting rules, and a test report template list of required information.
Figures 1 to 4 show example apparatus layouts for decomposition, distillation and combustion systems. Table 1 gives the tolerances used when comparing analytical values, and the annexes provide reference materials, round robin results and example ICP-OES spectral lines.
Relations
- Effective Date
- 15-Nov-2023
- Effective Date
- 12-Feb-2026
Frequently Asked Questions
EN ISO 17947-1:2026 is a standard published by the European Committee for Standardization (CEN). Its full title is "Fine ceramics (advanced ceramics, advanced technical ceramics) - Methods for chemical analysis of silicon nitride powders - Part 1: Wet chemical methods, X-ray fluorescence (XRF) using the fused cast-bead method, carrier-gas hot extraction (CGHE) and combustion methods (ISO 17947-1:2026)". This standard covers: This document specifies methods for the determination of silicon, nitrogen, aluminium, iron, calcium, oxygen, carbon, fluorine, and chlorine in silicon nitride powders. This document is applicable for the chemical analysis of silicon nitride powders used as raw material for fine ceramics.
This document specifies methods for the determination of silicon, nitrogen, aluminium, iron, calcium, oxygen, carbon, fluorine, and chlorine in silicon nitride powders. This document is applicable for the chemical analysis of silicon nitride powders used as raw material for fine ceramics.
EN ISO 17947-1:2026 is classified under the following ICS (International Classification for Standards) categories: 81.060.30 - Advanced ceramics. The ICS classification helps identify the subject area and facilitates finding related standards.
EN ISO 17947-1:2026 has the following relationships with other standards: It is inter standard links to EN ISO 17947:2023, ISO 17947-1:2026. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.
EN ISO 17947-1:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 4 Analytes and ranges
- 5 Preparation of test sample
- 5.1 General
- 5.2 Sampling
- 5.3 Drying
- 5.4 Weighing
- 6 Apparatus and reagents
- 7 Blank test
- 8 Determination of silicon
- 8.1 Classification of determination methods
- 8.2 Fusion-dehydration/insolubilization separation-gravimetry and ICP-OES
- 8.3 XRF using fused cast-bead method
- 9 Determination of nitrogen
- 9.1 Classification of determination methods
- 9.2 Acid pressure decomposition-distillation separation-acidimetric titration method
- 6 PTFE vessel
- 3 Dumet wire
- 9.3 Inert gas fusion-thermal conductivity method
- 9.4 Fusion-ammonia separation-acidimetric titration method
- 10 Determination of aluminium, iron, and calcium
- 10.1 Principle
- 10.2 Reagents
- 10.3 Apparatus
- 10.4 Procedure
- 10.5 Blank test
- 10.6 Calibration
- 10.7 Calculation
- 11 Determination of oxygen
- 11.1 Principle
- 11.2 Reagents
- 11.3 Apparatus
- 11.4 Instrument
- 11.5 Procedure
- 11.6 Blank test
- 11.7 Calculation of calibration coefficient
- 11.8 Calculation
- 12 Determination of carbon
- 12.1 Classification of determination methods
- 12.2 Combustion (induction furnace)-IR absorption spectrometry
- 9 IR spectrometer
- 12.3 Combustion (resistance furnace)-coulometry
- 12.4 Combustion (resistance furnace)-thermal conductivity
- 13 Determination of fluorine and chlorine
- 13.1 Principle
- 13.2 Reagents
- 13.3 Apparatus
- 13.4 Procedure
- 13.5 Blank test
- 13.6 Calibration
- 13.7 Calculation
- 14 Reporting analytical values
- 14.1 Number of analyses
- 14.2 Evaluation of analytical values
- 14.3 Expression of analytical values
- 15 Test report
- Annex A
- Annex B
- Annex C
- Bibliography
Introduction
[1] This document has been developed from Japanese Industrial Standard JIS R 1603:2007 with reference to [2] [3] CEN ENV 14226:2002 and ASTM C1494-01:2007 , and is applicable to the chemical analysis of silicon nitride raw powders for fine ceramics use. This document covers both major and minor constituents, such as silicon, nitrogen, and some trace metallic and non-metallic elements.
SIST EN ISO 17947-1:2027 International Standard ISO 17947-1:2026(en) Fine ceramics (advanced ceramics, advanced technical ceramics) — Methods for chemical analysis of silicon nitride powders — Part 1:
Wet chemical methods, X-ray fluorescence (XRF) using the fused cast-bead method, carrier-gas hot extraction (CGHE) and combustion methods
1 Scope
This document specifies methods for the determination of silicon, nitrogen, aluminium, iron, calcium, oxygen, carbon, fluorine, and chlorine in silicon nitride powders. This document is applicable for the chemical analysis of silicon nitride powders used as raw material for fine ceramics.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 2828, Aluminium oxide primarily used for the production of aluminium — Determination of fluorine content - Alizarin complexone and lanthanum chloride spectrophotometric method ISO 3696, Water for analytical laboratory use — Specification and test methods ISO 6353-1, Reagents for chemical analysis — Part 1: General test methods ISO 6353-2, Reagents for chemical analysis — Part 2: Specifications — First series ISO 6353-3, Reagents for chemical analysis — Part 3: Specifications — Second series ISO 8656-1, Refractory products — Sampling of raw materials and unshaped products — Part 1: Sampling scheme ISO 21068-2:2024, Chemical analysis of raw materials and refractory products containing silicon-carbide, silicon-nitride, silicon-oxynitride and sialon — Part 2: Determination of volatile components, total carbon, free carbon, silicon carbide, total and free silicon, free and surface silica ISO 21068-3:2024, Chemical analysis of raw materials and refractory products containing silicon-carbide, silicon-nitride, silicon-oxynitride and sialon — Part 3: Determination of nitrogen, oxygen and metallic and oxidic constituents ISO 21438-2, Workplace atmospheres — Determination of inorganic acids by ion chromatography — Part 2:
Volatile acids, except hydrofluoric acid (hydrochloric acid, hydrobromic acid and nitric acid) ISO 21438-3, Workplace atmospheres — Determination of inorganic acids by ion chromatography — Part 3:
Hydrofluoric acid and particulate fluorides
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en) ISO 26845:2008, Chemical analysis of refractories — General requirements for wet chemical analysis, atomic absorption spectrometry (AAS) and inductively coupled plasma atomic emission spectrometry (ICP-AES) methods
3 Terms and definitions
No terms and definitions are listed in this document.
ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- ISO Online browsing platform: available at https:// www .iso .org/ obp
- IEC Electropedia: available at https:// www .electropedia .org/
4 Analytes and ranges
Analytes and ranges specified in this document shall be as follows. a) Silicon (Si), range of 30 % to 70 % (mass fraction) b) Nitrogen (N), range of 30 % to 45 % (mass fraction) c) Aluminium (Al), range of 0,001 % to 0,6 % (mass fraction) d) Iron (Fe), range of 0,001 % to 0,6 % (mass fraction) e) Calcium (Ca), range of 0,001 % to 0,03 % (mass fraction) f) Oxygen (O), range of 0,05 % to 5 % (mass fraction) g) Carbon (C), range of 0,01 % to 6 % (mass fraction) h) Fluorine (F), range of 0,001 % to 0,2 % (mass fraction) i) Chlorine (Cl), range of 0,001 % to 0,2 % (mass fraction) NOTE The results of an interlaboratory test conducted using three silicon nitride powder samples are listed in Annex B.
5 Preparation of test sample
5.1 General
The method of preparing samples shall be in accordance with ISO 8656-1 unless otherwise mutually agreed upon between the analyser and the customer.
5.2 Sampling
Sampling shall be in accordance with ISO 8656-1.
5.3 Drying
The following procedure shall be used: Take about 10 g of the sample into a flat-type weighing bottle (60 mm × 30 mm) and spread it uniformly over the bottom of the bottle. Place the bottle in a drying oven at 110 °C ± 5 °C for 2 h without a lid, and then cool in a desiccator (desiccant: magnesium perchlorate for drying) with a lid for 1 h.
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en)
5.4 Weighing
The required quantity of the sample shall be weighed to the nearest 0,1 mg using a balance.
6 Apparatus and reagents
Unless otherwise specified for each determination, ordinary laboratory apparatus for chemical analysis as listed in ISO 26845:2008, Clause 4 may be used. Reagents shall conform to the requirements of ISO 6353-1, ISO 6353-2, and ISO 6353-3. Unless otherwise specified for each determination, reagents of analytical grade listed in ISO 26845:2008, Clause 5, shall be used.
7 Blank test
Blank test shall be carried out without the sample by using identical quantities of reagents, conditions, and procedures throughout each determination to correct the analytical values obtained.
8 Determination of silicon
8.1 Classification of determination methods
Silicon shall be determined by either of the following methods. If analytical results with four figures are required, use the method A. If analytical results with two or three figures are required, the method B can be used.
- Method A: Fusion–dehydration/insolubilization separation–gravimetry and inductively coupled plasma optical emission spectrometry (ICP-OES)
- Method B: XRF using fused cast-bead method
8.2 Fusion-dehydration/insolubilization separation-gravimetry and ICP-OES
8.2.1 Principle
A sample is fused with alkaline carbonate and the melt is treated with an acid to separate into two parts of silicon, insoluble silicon and soluble silicon, by filtration. Insoluble silicon is determined gravimetrically as silicon dioxide after ignition of the insoluble residue, whereas soluble silicon is determined in the filtrate using ICP-OES. The sum of them represents the content of silicon in the sample.
8.2.2 Reagents
Reagents of analytical grade shall be used. Reagent solutions shall be preserved in plastic bottles. 8.2.2.1 Water, of grade 1 or superior specified in ISO 3696.
8.2.2.2 Sodium carbonate, Na CO , anhydrous, specified in ISO 6353-3 or that of higher grade. 2 3 8.2.2.3 Hydrochloric acid (1+1), (1+4), (1+50), HCl, concentrated hydrochloric acid (c(HCl) = 32 %, mass fraction) diluted (1+1), (1+4) and (1+50) by volume with water (8.2.2.1). 8.2.2.4 Sulfuric acid (1+1), (1+4), H SO , concentrated sulfuric acid (c(H SO ) = 96 %, mass fraction) 2 4 2 4 diluted (1+1) and (1+4) by volume with water (8.2.2.1).
8.2.2.5 Cellulose powder.
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en)
8.2.2.6 Polyethylene glycol (PEG) solution, (C H O) H O, 0,05 % mass fraction of PEG, prepared by
2 4 n 2 dissolving solid PEG in water (8.2.2.1).
8.2.2.7 Hydrofluoric acid, HF, c(HF) = 48 %, mass fraction.
8.2.3 Apparatus and instruments
Ordinary laboratory apparatus and instruments for chemical analysis in accordance with ISO 26845:2008, 4 may be used.
8.2.3.1 Platinum dish.
8.2.3.2 Platinum crucible.
8.2.3.3 Burner, capable of heating at 1 100 °C.
8.2.3.4 Muffle furnace, capable of being operated at 1 100 °C. 8.2.3.5 Balance, readable to 0,1 mg.
8.2.3.6 Inductively coupled plasma optical emission spectrometer (ICP-OES).
8.2.4 Procedure
8.2.4.1 General
The procedure shall be as follows. The procedure described in ISO 21068-2:2024, Clause 8 may be alternatively used.
8.2.4.2 Fusion of sample
The following procedure shall be used: Weigh 0,30 g of the sample and 2,0 g of sodium carbonate, anhydrous, into a platinum dish and mix well. Start to heat carefully and increase the temperature gradually to 1 000 °C to completely fuse the sample using a burner or a muffle furnace.
8.2.4.3 Separation of silicon
The following procedure shall be used: Add 20 ml of hydrochloric acid (1+1) to dissolve the melt on a hot plate. Silicon dioxide will appear to be jellified and precipitated at this stage. There are two methods to separate the precipitated silicon dioxide.
a) Dehydrate carefully the precipitate to dryness in order to prevent it from spattering and add 5 ml of hydrochloric acid (1+1) and 20 ml of water to dissolve hydrochloric acid soluble components of the precipitate. Filtrate the precipitate with a filter paper and wash with hot hydrochloric acid (1+50) several times and then with hot water sufficiently until it contains no salt. Collect the filtrate and washings together in a volumetric flask and dilute to volume with water. Preserve this precipitate for gravimetry of insoluble silicon and the solution for the ICP-OES determination of soluble silicon, respectively. b) After formation of jellified silicon dioxide, add 0,05 g of cellulose powder and 10 ml of PEG solution (8.2.2.6) to agglomerate silicon dioxide for easy filtration. Filtrate and wash using the same procedure as described in a), and then preserve this precipitate for gravimetry of insoluble silicon and the solution for the ICP-OES determination of soluble silicon, respectively.
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en)
8.2.4.4 Gravimetry for insoluble silicon
The following procedure shall be used: Transfer the filter paper with the precipitate to a platinum crucible. Heat the platinum crucible slowly using a burner (8.2.3.3) or a muffle furnace (8.2.3.4) until complete ashing of the filter paper and then calcine the residue at 1 100 °C. Place the platinum crucible in a desiccator to cool to room temperature. Weigh the platinum crucible. Moisten the residue in the platinum crucible with a few drops of water (8.2.2.1) and sulfuric acid (1+1) (8.2.2.4) and add 10 ml of hydrofluoric acid (8.2.2.7). Then evaporate to dryness on a hot plate to remove all silicon dioxide, calcine the residue at 1 100 °C using a burner or in a muffle furnace and place the platinum crucible in a desiccator to cool to room temperature. Weigh the platinum crucible again. The loss of mass after hydrofluoric acid treatment corresponds to the amount of insoluble silicon dioxide.
8.2.4.5 ICP-OES for soluble silicon
The following procedure shall be used: Nebulize the test solution obtained in 8.2.4.3 into the plasma of an ICP-OES to determine soluble silicon in the sample.
NOTE An example for a suited silicon emission line is listed in Annex C.
8.2.5 Blank test
Blank determinations shall be performed according to 8.2.4.2 to 8.2.4.5 without the sample.
8.2.6 Calibration
For ICP-OES, calibration solutions shall be prepared to span the range of concentration of silicon in the test solution. Each calibration solution shall have a similar matrix to the test solution. With those calibration solutions, the calibration function for soluble silicon shall be created to establish the relation between the emission intensity measured with the test solution and the concentration of silicon in the test solution.
8.2.7 Calculation
With the amount of insoluble silicon (8.2.4.4), soluble silicon (8.2.4.5) and the blank test (8.2.5), the content of silicon shall be calculated according to Formula (1).
VAA
w mm 0,4674 (1)
Si 10
m
where w is the mass fraction of silicon in the sample, in percent; Si m is the mass of insoluble silicon dioxide in the sample (8.2.4.4), in grams;
m is the mass of insoluble silicon dioxide in the blank test (8.2.5), in grams;
A is the concentration of soluble silicon in the test solution (8.2.4.3), in milligrams per litre;
A is the concentration of soluble silicon in the blank solution (8.2.5), in milligrams per litre;
V is the volume of the test and blank solution, in millilitres; m is the mass of the sample (8.2.4.2), in grams.
8.3 XRF using fused cast-bead method
The procedure shall be in accordance with ISO 21068-3:2024, 8.2.
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en)
9 Determination of nitrogen
9.1 Classification of determination methods
Nitrogen shall be determined by either of the following methods. Methods A and C provide a higher precision than method B.
NOTE Based on practical experience, methods A and C provide a precision of two valid decimal places. Method B usually provides a precision of one valid decimal place.
- Method A: Acid pressure decomposition–distillation separation–acidimetric titration method
- Method B: Inert gas fusion–thermal conductivity method
- Method C: Fusion–ammonia separation–acidimetric titration method
9.2 Acid pressure decomposition-distillation separation-acidimetric titration method
9.2.1 Principle
The sample is decomposed in a pressure decomposition vessel with a mixture of hydrofluoric acid and sulfuric acid to convert nitrogen into ammonia. Boric acid is added and the solution is transferred into a distillation flask. After addition of sodium hydroxide, the ammonia is separated by steam distillation and the distillate is collected in a receiving vessel containing a known amount of amidosulfuric acid. The distilled ammonia reacts with amidosulfuric acid and the excess of amidosulfuric acid is back-titrated with a standardized sodium hydroxide solution.
9.2.2 Reagents
Reagents of analytical grade shall be used. Reagent solutions shall be preserved in plastic bottles. 9.2.2.1 Water, of grade 1 or superior specified in ISO 3696.
9.2.2.2 Hydrofluoric acid, HF, c(HF) = 48 %, mass fraction.
9.2.2.3 Sulfuric acid (1+1), H SO , concentrated sulfuric acid (c(H SO ) = 96 %, mass fraction) diluted 2 4 2 4 (1+1) by volume with water (9.2.2.1).
9.2.2.4 Sodium hydroxide, NaOH, more than 97,0 % (mass fraction) of purity.
9.2.2.5 Sodium hydroxide solution (500 g/l), prepared by dissolving sodium hydroxide (9.2.2.4) in
water (9.2.2.1).
9.2.2.6 Amidosulfuric acid, H NO S, more than 99,0 % (mass fraction) of purity. 3 3 9.2.2.7 0,1mol/l amidosulfuric acid solution, prepared by dissolving amidosulfuric acid (9.2.2.6) in water (9.2.2.1). Weigh 10,0 g of amidosulfuric acid into a 1 000 ml volumetric flask, dissolve in approximately
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en) 200 ml water, dilute with water to volume and mix well. The factor of this solution shall be calculated according to Formula (2).
F = m × P/(9,709 5 × 100) (2) where F is the factor of the 0,1 mol/l amidosulfuric acid solution; m is the mass of amidosulfuric acid, g; P is the purity of amidosulfuric acid, % (mass fraction).
9.2.2.8 0,1 mol/l sodium hydroxide solution, prepared by dissolving sodium hydroxide (9.2.2.4) in water (9.2.2.1). Weigh 4,0 g of sodium hydroxide into a 1 000 ml volumetric flask, dissolve in approximately 200 ml water, dilute with water to volume and mix well.
The factor of this solution shall be determined using the following procedure: Pour exactly 50 ml of the 0,1 mol/l amidosulfuric acid solution into a beaker (200 ml) and dilute with water to about 100 ml. Titrate this solution with the 0,1 mol/l sodium hydroxide solution using a pH meter. Take the end point as pH 5,5 and determine the volume of the titrant consumed. The factor of this solution shall be calculated according to Formula (3).
F = F × 50,00/V (3)
where F is the factor of the 0,1 mol/l sodium hydroxide solution;
F is the factor of the 0,1 mol/l amidosulfuric acid solution; V is the titration volume of the 0,1 mol/l sodium hydroxide solution, ml. 9.2.2.9 Boric acid, H BO .
3 3 9.2.2.10 Ammonium sulfate, (NH ) SO , more than 99,9 % (mass fraction) of purity. 4 2 4
9.2.3 Apparatus
Ordinary laboratory apparatus for chemical analysis shall be used and the following. 9.2.3.1 Platinum crucible.
9.2.3.2 Pressure decomposition vessel, commercially available. An example is shown in Figure 1. Since hydrofluoric acid under high temperature and pressure is used for sample decomposition, polytetrafluoroethylene (PTFE) shall be used for vessel and cap (see Figure 1). Instead of PTFE, caps and vessels made of perfluoroalkoxy (PFA) may be used. The vessels shall be exclusively used for the determination of nitrogen according to method A (9.1) to avoid cross-contamination by nitrogen. If vessels are used that have ever come into contact with nitric acid, lower values of nitrogen can be obtained.
9.2.3.3 Drying Oven, capable of heating at 160 °C ± 5 °C.
9.2.3.4 Steam distillation apparatus, consisting of the components listed below. An example of the
apparatus is shown in Figure 2. Each component shall be made of hard glass coupled by common ground joints and fixed by springs or clamps.
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en) Dimensions in millimetres Key 1 centre screw 2 screw cap 3 top plate 4 polytetrafluoroethylene (PTFE) cap 5 pressure vessel
6 PTFE vessel
7 bottom plate Figure 1 — An example of sealed decomposition vessel
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en) Dimensions in millimetres Key a flask (2,5 l) for generation of steam b trap (500 ml) c sphere and tube d distillation flask (750 ml) e Graham condenser f receiver 1 funnel 2 ball joint
3 Dumet wire
4 funnel with stopcock 5 rubber tube 6 13 to15 coils 7 small holes 8 electric heater 9 connection of rubber tube with pinchcock 10 jack Figure 2 — An example of steam distillation apparatus
SIST EN ISO 17947-1:2027 ISO 17947-1:2026(en) 9.2.3.5 Steam generation flask (2,5 l), equipped with a funnel with a cock, an immersion heater (with 1 kW Nichrome wire), and a steam outlet tube.
9.2.3.6 Trap, the bottom of a bulb shall be connected to a rubber tube with a pinch cock for a drain. The tip of steam leading-out tube shall have several small holes. 9.2.3.7 Bulb, equipped with a steam leading-in tube, a funnel with a cock, a splash-proof trap, etc. The steam leading-in tube shall be cut in the middle enabling the exchange of the tip by connecting to a rubber tube.
9.2.3.8 Distillation flask (750 ml).
9.2.3.9 Coiled condenser.
9.2.3.10 Receiver, a tall beaker (300 ml) shall be used.
9.2.3.11 pH meter, readable to the smallest value of 0,1 equipped with a glass electrode.
9.2.4 Procedure
The following procedures shall be used:
a) Acid pressure decomposition of the sample. Weigh 0,15 g of the sample into a platinum crucible (20 ml) and add 5 ml of sulfuric acid (1+1) and 5 ml of hydrofluoric acid. Place the crucible into a pressure decomposition vessel and close the vessel according to the manufacturer’s instructions. If an antistatic device is available during weighing, the sample may be directly weighed into the PTFE vessel (see Figure 1). Place the vessel into a drying oven and heat at 160 °C ± 5 °C for 16 h. Acid pressure decomposition under microwave irradiation may be performed if available. For microwave sample decomposition the sample shall be weighed into a PTFE crucible or directly into the PTFE vessel of the decomposition system (see Figure 1).
b) Preparation of the sample solution. After cooling, disassemble the vessel. Transfer the solution into a 100 ml plastic beaker, thoroughly rinse the crucible or the PTFE vessel with water and add the rinse water to the beaker. Add 5 g of boric acid and mix well.
...