ISO 18756:2003
(Main)Fine ceramics (advanced ceramics, advanced technical ceramics) — Determination of fracture toughness of monolithic ceramics at room temperature by the surface crack in flexure (SCF) method
- Abstract
ISO 18756:2003 describes a test method that covers the determination of fracture toughness of monolithic ceramic materials at room temperature by the surface crack in flexure (SCF) method. This International Standard is intended for use with monolithic ceramics and whisker- or particulate-reinforced ceramics that are regarded as macroscopically homogeneous. It does not include continuous-fiber reinforced ceramic composites. The test method is applicable to materials with either flat or rising crack growth resistance curves.
- Status
- Published
- Publication Date
- 27-Nov-2003
- Technical Committee
- ISO/TC 206 - Fine ceramics
- Current Stage
- 9093 - International Standard confirmed - 90 Review
- Start Date
- 25-Sep-2025
Buy Documents
ISO 18756:2003 - Fine ceramics (advanced ceramics, advanced technical ceramics) — Determination of fracture toughness of monolithic ceramics at room temperature by the surface crack in flexure (SCF) method Released:11/28/2003
ISO 18756:2003 - Céramiques techniques — Détermination de la ténacité a la rupture des céramiques monolithiques a température ambiante par fissuration superficielle en flexion Released:4/11/2005
Overview
ISO 18756:2003 specifies the surface crack in flexure (SCF) test method for determining the fracture toughness of monolithic and whisker- or particulate-reinforced advanced ceramics at room temperature. The method uses a small, semi‑elliptical surface precrack produced by a Knoop indentation, followed by fracture in four‑point flexure and fractographic measurement of the critical crack size to calculate the SCF fracture toughness value (KIsc). The standard is intended for macroscopically homogeneous ceramics and excludes continuous‑fiber reinforced ceramic composites.
Key topics and requirements
- Scope & applicability: Monolithic ceramics and whisker/particulate‑reinforced ceramics; suitable for materials with flat or rising R‑curve behavior. Note: usually applicable to materials with fracture toughness ≲ ~10 MPa·m^0.5; may be difficult for very hard/soft or porous materials.
- Precrack method: Knoop indentation is used to generate a small surface crack; residual indentation stresses are removed by careful polishing before fracture.
- Test geometry & fixtures: Rectangular beam specimens tested in four‑point flexure (1/3 or 1/4 span configurations) in accordance with ISO 14704.
- Apparatus & measurement:
- Universal test machine meeting ISO 7500‑1 Class 1 accuracy.
- Hardness tester capable of 20–50 N to create indentations.
- Micrometer or equivalent with 0.002 mm resolution.
- Optical or SEM microscopy (typically 100×–500×) and dye penetrants for crack detection.
- Procedure essentials: make indentation, remove residual stresses, fracture in four‑point bending, perform fractography to measure precrack/critical crack, compute KIsc from fracture load and crack geometry.
- Annexes: guidance on environmental effects, precrack characterization, R‑curve estimation, and chamfer correction factors.
Practical applications and users
ISO 18756:2003 is used for:
- Material development and comparison of advanced ceramics.
- Quality assurance and incoming inspection of ceramic parts.
- Generating design and reliability data (fracture toughness inputs for design).
- Failure analysis and research into crack‑growth resistance (R‑curve behavior).
Typical users: materials scientists, ceramics engineers, R&D laboratories, quality control/QA labs, and standards bodies involved in advanced technical ceramics testing.
Related standards
- ISO 14704 - flexural strength of monolithic ceramics (fixture and specimen requirements)
- ISO 7500‑1 - verification and calibration of force‑measuring systems
- ISO 3611 - micrometer callipers (dimension measurement)
ISO 18756:2003 provides a practical, standardized SCF method to obtain reproducible fracture toughness data for monolithic advanced ceramics, supporting material selection, comparison, and engineering design.
Buy Documents
ISO 18756:2003 - Fine ceramics (advanced ceramics, advanced technical ceramics) — Determination of fracture toughness of monolithic ceramics at room temperature by the surface crack in flexure (SCF) method Released:11/28/2003
ISO 18756:2003 - Céramiques techniques — Détermination de la ténacité a la rupture des céramiques monolithiques a température ambiante par fissuration superficielle en flexion Released:4/11/2005
Frequently Asked Questions
ISO 18756:2003 is a standard published by the International Organization for Standardization (ISO). Its full title is "Fine ceramics (advanced ceramics, advanced technical ceramics) — Determination of fracture toughness of monolithic ceramics at room temperature by the surface crack in flexure (SCF) method". This standard covers: ISO 18756:2003 describes a test method that covers the determination of fracture toughness of monolithic ceramic materials at room temperature by the surface crack in flexure (SCF) method. This International Standard is intended for use with monolithic ceramics and whisker- or particulate-reinforced ceramics that are regarded as macroscopically homogeneous. It does not include continuous-fiber reinforced ceramic composites. The test method is applicable to materials with either flat or rising crack growth resistance curves.
ISO 18756:2003 describes a test method that covers the determination of fracture toughness of monolithic ceramic materials at room temperature by the surface crack in flexure (SCF) method. This International Standard is intended for use with monolithic ceramics and whisker- or particulate-reinforced ceramics that are regarded as macroscopically homogeneous. It does not include continuous-fiber reinforced ceramic composites. The test method is applicable to materials with either flat or rising crack growth resistance curves.
ISO 18756:2003 is classified under the following ICS (International Classification for Standards) categories: 81.060.30 - Advanced ceramics. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO 18756:2003 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
INTERNATIONAL ISO
STANDARD 18756
First edition
2003-12-01
Fine ceramics (advanced ceramics,
advanced technical ceramics) —
Determination of fracture toughness of
monolithic ceramics at room temperature
by the surface crack in flexure (SCF)
method
Céramiques techniques — Détermination de la ténacité à la rupture des
céramiques monolithiques à température ambiante par fissuration
superficielle en flexion
Reference number
©
ISO 2003
PDF disclaimer
This PDF file may contain embedded typefaces. In accordance with Adobe's licensing policy, this file may be printed or viewed but
shall not be edited unless the typefaces which are embedded are licensed to and installed on the computer performing the editing. In
downloading this file, parties accept therein the responsibility of not infringing Adobe's licensing policy. The ISO Central Secretariat
accepts no liability in this area.
Adobe is a trademark of Adobe Systems Incorporated.
Details of the software products used to create this PDF file can be found in the General Info relative to the file; the PDF-creation
parameters were optimized for printing. Every care has been taken to ensure that the file is suitable for use by ISO member bodies. In
the unlikely event that a problem relating to it is found, please inform the Central Secretariat at the address given below.
© ISO 2003
All rights reserved. Unless otherwise specified, no part of this publication may be reproduced or utilized in any form or by any means,
electronic or mechanical, including photocopying and microfilm, without permission in writing from either ISO at the address below or
ISO's member body in the country of the requester.
ISO copyright office
Case postale 56 • CH-1211 Geneva 20
Tel. + 41 22 749 01 11
Fax + 41 22 749 09 47
E-mail copyright@iso.org
Web www.iso.org
Published in Switzerland
ii © ISO 2003 — All rights reserved
Contents Page
Foreword. iv
1 Scope. 1
2 Normative references . 1
3 Terms and definitions. 1
4 Symbols . 3
5 Principle . 4
6 Apparatus. 5
7 Test specimens . 6
7.1 Specimen size, preparation and edge chamfering . 6
7.2 Number of specimens. 6
8 Procedure. 7
8.1 Introduction of the precrack by Knoop indentation . 7
8.2 Specimen fracture. 11
8.3 Crack size measurement. 12
8.4 Environmental effects. 13
8.5 Optional: Estimate of R-curve behaviour .14
8.6 Optional: Reference materials . 14
9 Calculation. 14
10 Test report. 15
Annex A (informative) Environmental effects. 17
Annex B (normative) Precrack characterization . 18
Annex C (informative) R-curve estimation by the SCF method. 25
Annex D (normative) Chamfer correction factors. 27
Bibliography . 29
Foreword
ISO (the International Organization for Standardization) is a worldwide federation of national standards bodies
(ISO member bodies). The work of preparing International Standards is normally carried out through ISO
technical committees. Each member body interested in a subject for which a technical committee has been
established has the right to be represented on that committee. International organizations, governmental and
non-governmental, in liaison with ISO, also take part in the work. ISO collaborates closely with the
International Electrotechnical Commission (IEC) on all matters of electrotechnical standardization.
International Standards are drafted in accordance with the rules given in the ISO/IEC Directives, Part 2.
The main task of technical committees is to prepare International Standards. Draft International Standards
adopted by the technical committees are circulated to the member bodies for voting. Publication as an
International Standard requires approval by at least 75 % of the member bodies casting a vote.
Attention is drawn to the possibility that some of the elements of this document may be the subject of patent
rights. ISO shall not be held responsible for identifying any or all such patent rights.
ISO 18756 was prepared by Technical Committee ISO/TC 206, Fine ceramics.
iv © ISO 2003 — All rights reserved
INTERNATIONAL STANDARD ISO 18756:2003(E)
Fine ceramics (advanced ceramics, advanced technical
ceramics) — Determination of fracture toughness of monolithic
ceramics at room temperature by the surface crack in flexure
(SCF) method
1 Scope
This International Standard describes a test method that covers the determination of fracture toughness of
monolithic ceramic materials at room temperature by the surface crack in flexure (SCF) method.
This International Standard is intended for use with monolithic ceramics and whisker- or particulate-reinforced
ceramics that are regarded as macroscopically homogeneous. It does not include continuous-fibre reinforced
ceramic composites.
The test method is applicable to materials with either flat or rising crack growth resistance curves. This
method is similar to ISO 15732 except that precracks are smaller and are made by a different procedure. The
methods should produce similar or identical results for materials with a flat R-curve.
1/2
NOTE This test method is usually applicable to ceramic materials with a fracture toughness less than ≈ 10 MPa m . It
may be difficult to form precracks with a Knoop indenter for materials with greater fracture toughness or those materials
which are soft (low hardness) such as some zirconias, or for porous ceramics.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated
references, only the edition cited applies. For undated references, the latest edition of the referenced
document (including any amendments) applies.
ISO 3611:1978, Micrometer callipers for external measurement
1)
ISO 7500-1:— , Metallic materials — Verification of static uniaxial testing machines — Part 1: Tension/
compression testing machines — Verification and calibration of the force-measuring system
ISO 14704:2000, Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for flexural
strength of monolithic ceramics at room temperature
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply.
1) To be published. (Revision of ISO 7500-1:1999)
3.1
stress intensity factor
K
I
magnitude of the elastic stress field singularity at the tip of a crack subjected to opening mode displacement
NOTE It is a function of applied force and test specimen size, geometry and crack length, and has dimensions of
force times length to the power of three over two.
3.2
fracture toughness
generic term for measures of resistance of extension of a crack
3.3
fracture toughness value
K
Isc
fracture toughness value measured by the SCF method
NOTE This is the measured stress intensity factor corresponding to the crack extension resistance of a semi-elliptical
small crack formed underneath a Knoop indentation. The measurement is performed to the operational procedure herein
and satisfies all the validity requirements.
3.4
precrack
crack introduced into the test specimen artificially prior to testing the specimen to fracture
3.5
crack front line
line to indicate the position of the tip of the crack
3.6
critical stress intensity factor
K
Ic
critical value of K at which fast fracture occurs
I
3.7
critical crack
crack at fracture at maximum load and whose stress intensity factor just reaches the critical stress intensity
factor
3.8
critical crack size
size of the critical crack at fracture
NOTE The critical crack will be larger than the precrack if stable crack extension occurs due to environmentally-
assisted slow crack growth or rising R-curve behaviour.
3.9
four-point 1/4-point flexure
specific configuration of four-point flexural strength testing where the inner bearings are situated one quarter
of the support span away from the two outer bearings
3.10
four-point 1/3-point flexure
specific configuration of four-point flexural strength testing where the inner bearings are situated one third of
the support span away from the two outer bearings
3.11
flexural strength
maximum nominal stress at fracture of a specified elastic beam loaded in bending
2 © ISO 2003 — All rights reserved
4 Symbols
a Crack depth
A Flexure fixture moment arm
B Specimen width, the cross section dimension perpendicular to the direction of loading in bending
c Crack half width
C Chamfer size
d Length of Knoop indentation long diagonal
h Depth of Knoop indentation
F Knoop indentation load
F Chamfer correction factor
c
H (a/c, a/W) A polynomial in the stress intensity factor coefficient, for the point on the crack periphery where it
intersects the specimen surface
H (a/c, a/W) A polynomial in the stress intensity factor coefficient, for the deepest part of the surface crack
K Stress intensity factor, Mode I
I
K Critical stress intensity factor, Mode I
Ic
K Fracture toughness value, surface crack in flexure method
Isc
L Flexure fixture support span
L Specimen length
T
M (a/c, a/W) A polynomial in the stress intensity factor coefficient
P Load at fracture
Q (a/c) A polynomial function of the surface crack ellipticity
S (a/c, a/W) Factor in the stress intensity factor coefficient
W Specimen depth, the cross section dimension parallel to the direction of loading in bending
Y Stress intensity factor coefficient
Y Stress intensity factor coefficient at the deepest part of the surface crack
d
Y The maximum stress intensity factor coefficient along the boundary of the surface crack
max
Y Stress intensity factor coefficient at the intersection of the surface crack with the specimen
s
surface
5 Principle
This International Standard is for material development, material comparison, quality assurance,
characterization, reliability, and design data generation. The method determines the fracture toughness value,
K by fracturing a common flexure specimen which has a small surface precrack (see Figure 1). The
Isc
specimen is indented with a Knoop indenter in order to make a small, semi-elliptical surface crack. The
specimen is polished or ground carefully until the indentation and associated residual stress field are removed.
The specimen is fractured in four-point flexure. The fracture toughness, K , is calculated from the fracture
Isc
load and the measured critical crack size. Fractography is required to measure the precrack size and to
determine whether the crack has grown in size. Fracture toughness as a function of crack size may be
evaluated by varying the Knoop indentation load that is used to make the precrack. Background information
concerning this test method may be found in References [1] and [2]. An international interlaboratory
comparison study (round robin) project on this method is described in References [3], [4] and [5].
If the ceramic is too soft (low hardness) or has too great a fracture toughness, it may be difficult to create a
precrack by the SCF method. In addition, for some materials (particularly those with coarse grain or
heterogeneous microstructures), it may be difficult to detect the crack on the fracture surface. If the user is not
sure of the applicability of this method, then a single trial specimen may be tested with an abbreviated
procedure. Indent the specimen and fracture it without removal of the indentation and residual stresses.
Inspect the fracture surface to confirm that the specimen fractured from the precrack (and not from a material
flaw) and that the precrack can be detected on the fracture surface.
Precracking is by Knoop indentation only in this International Standard. Residual stresses underneath the
indentation are removed in this test method. There is some limited experience with SCF precracking by Vickers
indentation [3, 4, 5, 6, 7]
Key
1 indentation and precrack
2 polished or lapped surface
Figure 1 — Indentation and precrack in a flexural specimen
4 © ISO 2003 — All rights reserved
6 Apparatus
6.1 Testing machine, capable of applying a uniform cross-head speed. The testing machine shall be in
accordance with ISO 7500-1:— Class 1 with an accuracy of 1 % of indicated load at fracture.
6.2 Flexural fixtures, four-point as shown in Figure 2. Flexural fixtures shall meet the requirements of
ISO 14704.
The fixtures shall either be semi-articulating or fully-articulating depending upon the condition of the specimens.
If the specimens meet the parallelism requirements of 7.1, then semi-articulating fixtures may be used. Semi-
articulating fixtures are usually completely satisfactory for machined specimens. If the specimens do not meet
the parallelism requirements of 7.1 (due to hand grinding unevenness, problems with machining, or other
causes), then fully-articulating fixtures shall be used. Fully-articulating fixtures also may be used with machined
specimens. Specimens shall be loaded and supported by bearings. The bearings shall be free to roll in order to
eliminate friction. For four-point flexure, the two inner bearings shall be free to roll inwards, and the two outer
bearings shall be free to roll outwards.
Four-point 1/4-point fixtures with 20 mm support span and 10 mm inner span are also permitted. Such fixtures
shall meet the requirements of ISO 14704.
Dimensions in millimetres
L = 40,0 ± 0,10 or L = 20,0 ± 0,10
a) Four-point 1/4-point flexure
L = 30,0 ± 0,10
b) Four-point 1/3-point flexure
Key
1 loading bearings
2 support bearings
Figure 2 — Four-point flexure
6.3 Micrometer, such as described in ISO 3611 but with a resolution of 0,002 mm shall be used to
measure the specimen dimensions. The micrometer shall have flat anvil faces such as shown in ISO 3611.
The micrometer shall not have a ball tip or sharp tip since these might damage the specimen. Alternative
dimension measuring instruments may be used provided that they have a resolution of 0,002 mm or finer.
6.4 Hardness testing machine, conventional type, to create the Knoop indentation. The machine shall be
able to apply loads of 20 N to 50 N or greater. If a hardness machine with this load range is not available, then
a strength testing machine (6.1) may be used although some loss of accuracy or control of indentation and
crack size may result.
6.5 Microscopes, optical and/or scanning electron, shall be used to detect the precrack (or critical crack)
and measure its size on the specimen fracture surface after the test. Magnifications of 100× to 500× are
usually required. The microscope shall be capable of making photographic or digital records of the cracks.
6.6 Dye penetrants, to highlight the crack. Dye penetrants that do not promote slow crack growth nor bleed
(spread on the fracture surface after fracture) are preferred.
6.7 Temperature measuring device, a thermometer or other device to measure ambient temperature
during the fracture of the specimen.
6.8 Humidity measuring device, such as a hygrometer, sling psychrometer, or other device to measure
ambient humidity during the fracture of the specimen.
7 Test specimens
7.1 Specimen size, preparation and edge chamfering
7.1.1 Rectangular beam specimens with dimensions as shown in Figure 3 shall be used. The cross-
sectional tolerances are ± 0,2 mm. The parallelism tolerance on opposite longitudinal faces is 0,015 mm.
7.1.2 Specimens shall be prepared in accordance with ISO 14704 with the exceptions noted below. The
indentation may be placed in either a 3 mm or 4 mm wide face. A diamond-grit wheel 320 or finer shall be
used to remove the last 0,04 mm on the surface that is used for the indentation. This surface shall be polished,
lapped or fine ground to provide a flat, smooth surface for the surface crack.
NOTE The surface does not require a polished, high-quality finish such as required for a hardness measurement. The
surface need only be flat so that the Knoop indentation is not affected by machining striations or marks, or specimen
unevenness.
7.1.3 Chamfers or edge rounds are optional. If premature fracture occurs from edge damage, then the
edges shall be chamfered or rounded as specified in ISO 14704. The chamfer size should be 0,15 mm or less.
See Figure 3.
7.2 Number of specimens
The number of specimens shall be not less than five. It is recommended that at least ten specimens be
prepared. This will provide specimens for practice tests to determine the best indentation loads and provide
specimens to make up for unsuccessful or invalid tests. More specimens are needed if environment, testing
rate, or precrack sizes are to be varied.
6 © ISO 2003 — All rights reserved
Dimensions in millimetres
L W 25 for 20 mm test fixtures or
T
L W 35 for 30 mm test fixtures or
T
L W 45 for 40 mm test fixtures
T
a
Edge chamfers or rounding.
Figure 3 — Test specimen dimensions
8 Procedure
8.1 Introduction of the precrack by Knoop indentation
8.1.1 Use a Knoop indenter to indent the middle of the polished, lapped or fine ground surface of the
o
specimen. The indentation shall be perpendicular to the specimen long axis to within 2 as shown in Figure 1.
o o
One end of the specimen shall be tilted approximately 0,25 to 0,5 as shown in Figure 4. A full load dwell time
of 15 s or more during the indentation cycle shall be used. The indentation may be placed in either a 3 mm or
4 mm wide face as shown in Figure 5. It is recommended that the indentation be placed near to the exact
centre of the surface, both along the width dimension B and along the specimen length, in order to make it
easy to confirm that fracture occurs from the precrack.
NOTE 1 The 0,25° to 0,5° tilt makes the precrack easier to detect on the fracture surface. The specimen tilt causes
precrack tilts from 0° to 5°.
NOTE 2 In some instances such as with zirconia, indentation times longer than 15 s may be helpful.
NOTE 3 A trial specimen may be tested to help determine the best indentation load. Indent then fracture the specimen
in the flexure fixtures without removal of the indentation and residual stress damage zone. Examine the fracture surface to
confirm that the specimen has fractured from the precrack, that the precrack is discernible, and within the prescribed size
limits.
NOTE 4 The Knoop indentation procedure to create a surface crack will not be successful on very soft or porous
ceramics since a precrack will not form under the indentation. The process may not work on very tough ceramics which
are resistant to the formation of cracks, or where the cracks are very small and likely to be removed during the subsequent
polishing step to remove the residual stress and damage zone.
a) Specimen side view b) Specimen end view
Key
1 Knoop indenter
2 precrack
3 indent with precrack
4 platform tilts specimen
Figure 4 — Indentation of the precrack by Knoop indentation
NOTE 1 The indentation may be placed on either the wide 4 mm face or the narrow 3 mm face.
NOTE 2 The crack size has been exaggerated for illustrative purposes and is usually much smaller.
Figure 5 — Specimen cross section
8.1.2 The optimum indentation load used may have to be determined for each different class of material by
the use of a few trial specimens. The load shall be sufficient to create a crack that is larger than the naturally-
occurring flaws in the material, but not too large relative to the specimen cross section size (2c < 0,5B and
a < 0,5W) nor so large that the indentation is badly spalled or shattered. Indentation loads of approximately
20 N are suitable for very brittle ceramics, 25 N to 50 N for medium tough ceramics, and 49 to 98 N for very
tough ceramics or ceramics with some porosity. Indentation loads of 98 N to 147 N may be necessary for
materials with medium- to coarse-grain sizes. In such materials, it is necessary to make large precracks that
will stand out against the normal microstructural roughness on the fracture surface.
8.1.3 Measure the length of the long diagonal, d, of the Knoop impression to within 0,005 mm (5 µm).
8 © ISO 2003 — All rights reserved
NOTE A conventional microhardness machine (6.4) may be used for this measurement. The measurement does not
require the precision needed for hardness measurements. If the Knoop hardness is reported, greater care is
recommended in making the diagonal size measurement and in the preparation of the initial specimen surface.
8.1.4 Compute the depth, h, of the Knoop impression as follows:
hd= /30 (1)
8.1.5 Measure the specimen depth, W, in the middle of the specimen at the indent location to within
0,002 mm. A hand micrometer (6.3) with vernier graduations marked in 0,002 mm increments is suitable.
8.1.6 Mark the side of the specimen with a pencil or other marker with an arrow to indicate which surface
has the precrack.
8.1.7 Remove the indentation and the residual stress damage zone.
8.1.7.1 Remove from the indented surface an amount of material that is approximately equal to 4,5h to
5,0h as shown in Figure 6. The material removal process shall not induce residual stresses or excessive
machining damage in the specimen surface. Be careful to remove material from the correct face. Mark with
pencil or permanent marker the faces that will not be ground or polished. Material may be removed by any
one of the three procedures described in 8.1.7.2, 8.1.7.3 and 8.1.7.4.
NOTE The removal of 4,5h to 5,0h eliminates the residual stress damage zone under the impression, and usually will
leave a precrack shape that has the greatest stress intensity factor at the deepest part of the precrack periphery. The
location of the maximum stress intensity can be controlled by the amount of material removed. The initial precrack under
the Knoop indent is roughly semicircular and the maximum Y, stress intensity factor coefficient, Y is at the surface. As
max
material is removed, the precrack becomes more semi-elliptical in shape (or like a section of a circle) and Y will shift to
max
the deepest part of the precrack. If too much material is removed, the remaining precrack will be too small and fracture will
not occur from the precrack. In such cases it is preferable to remove smaller amounts, provided that no less than 3h is
removed. If this step is not adequate to ensure fracture from the precrack, then a greater indentation load may be needed.
Key
1 material to be removed after indentation
NOTE The precrack extends below the Knoop hardness indentation, which has a depth h.
Figure 6 — The indentation and the residual stress damage zone
8.1.7.2 Material may be removed by hand grinding, hand lapping or hand polishing with abrasive papers
under wet or dry conditions. Hand polishing the specimen with 180 to 220 grit silicon carbide paper can
remove the required amount in 5 min to 10 min per specimen for many ceramics. Check the specimen height
frequently during this process. Remove the last 0,005 mm with a finer grit (220 to 280 grit) paper with less
pressure, so as to minimize polishing damage. Monitor the specimen depth, W, frequently during the material
removal step, with special emphasis on monitoring the evenness of the material removal.
Hand grinding, hand lapping or hand polishing may not be effective with very hard ceramics. For very hard
ceramics, material may be removed by machine polishing or lapping (8.1.7.3), or by machine surface grinding
(8.1.7.4).
Regularly change the orientation of the surface being hand polished or ground during material removal in
order to minimize unevenness. Unevenness may cause misalignments during subsequent flexure testing or
cause errors in the cross section size measurements.
NOTE 1 Dry hand grinding may be faster than wet grinding. Diamond impregnated polishing discs (30 µm) are also
effective in removing material by hand grinding.
NOTE 2 Hand lapping or grinding may make the precracked surface uneven or not parallel to the opposite specimen
surface. A slight rounding of the specimen edges is usually inconsequential.
NOTE 3 Finer grit (320 to 500 grit) papers are recommended for glasses for both rough removal and fine finishing steps
CAUTION — Fine ceramic powders or fragments may be created if the lapping or hand sanding is
done dry. Masks should be used or the removal done wet if there is an inhalation hazard, especially if
the ceramic contains silica or fine whiskers.
8.1.7.3 Material may be removed by machine polishing or lapping with diamond slurry or paste containing
about 0,3 µm particles. This requires about 10 min to 15 min per specimen for many ceramics. A trial
specimen may be polished to obtain an appropriate removal rate by adjusting applied masses, rotating speed
of the disc and polishing times in order to obtain the correct amount of material removal.
8.1.7.4 Material may be removed by surface grinding with diamond wheels on a grinding machine for
very hard materials. Take care to ensure that the correct amount of material has been removed from each
specimen. Avoid aggressive grinding conditions that may introduce residual stresses. If machine surface
grinding is used, fine wheel grits (320 to 600 grit) and small removal rates are recommended. Grinding may be
carried out under wet conditions.
8.1.7.5 After the prescribed amount of material has been removed, examine the ground-indented surface
for evidence of remnant lateral cracks. Figure 7 provides guidance. A low power reflected light metallurgical
optical microscope (6.5) with magnifications from 100× to 500× may be used to examine the ground-indented
tensile surface. If there is evidence of remnants of lateral cracks, then additional material should be removed
(6h to 10h) to ensure that the lateral cracks remnants are removed.
1/2
NOTE Deeper than normal lateral cracks may occur in materials with very low fracture toughness (< 3,0 MPa m ) or
if larger indentation loads (W 98 N) are used.
a) shows the ground surface after material removal. The Knoop indentation (dashed lines) has been removed and the
median crack is very tight and not visible. There are no traces of lateral cracks.
b) to e) show examples of remnants of lateral cracks which should be removed in accordance with 8.1.7.4 and 8.1.7.5.
Figure 7 — A ground surface and remnants of lateral cracks existing after removal of the damage zone
in some brittle materials
10 © ISO 2003 — All rights reserved
8.1.7.6 Annealing or heat treating to remove the residual stresses under the indentation is not permitted
by this International Standard due to the risk of crack tip blunting or crack healing.
8.1.8 Dry the specimen prior to testing if the material removal is done wet.
NOTE There is no consensus on the best conditions for drying specimens. Heating in an air or vacuum oven at
100 °C to 150 °C for times up to 1 h and then storage in a desiccator prior to testing may be sufficient.
8.1.9 If necessary, a dye penetrant (6.6) may be applied to aid crack detection. If a dye penetrant is used,
the specimen should be dried thoroughly prior to fracture.
8.1.10 Measure and record the specimen dimensions, B and W, in the vicinity of the precrack to within
0,002 mm.
8.2 Specimen fracture
8.2.1 Ensure that the specimen is dry.
8.2.2 Test the precracked specimens to fracture in four-point flexure in laboratory ambient conditions. If the
material is susceptible to slow crack growth, it is recommended that the testing conditions of 8.4 be applied.
NOTE Many oxides, glasses and ceramics having glassy boundary phases may be susceptible to slow crack growth.
Measured fracture toughness may be sensitive to displacement rate and moisture in the atmosphere. See Annex A for
additional background information.
8.2.3 Insert the specimen into the flexure fixture as shown in Figure 8, with the surface crack on the tension
face, approximately in the middle (within 1 mm) of the two inner loading rollers. The specimen may be
preloaded to no more than 25 % of the expected fracture load. Place cotton, crumpled tissue or other
appropriate material under the specimen to prevent the pieces from impacting the fixture upon fracture and to
prevent the fracture surface from being damaged by impact after the specimen breaks. Place a simple shield
around the fixture to ensure operator safety and to preserve the primary fracture pieces for subsequent
fracture analysis. If the specimen precracked face is not parallel to the opposite face to within 0,015 mm, then
fully-articulating fixtures shall be used.
8.2.4 Use a standard displacement rate of 0,5 mm/min for specimens tested with 30 mm or 40 mm support
span fixtures. Use a displacement rate of 0,10 mm/min to 0,13 mm/min for specimens tested with 20 mm
support span fixtures.
8.2.5 Apply a compressive load to the fixture until the specimen fractures. Measure the fracture load to an
accuracy of ± 1 %. The time to fracture should not exceed 20 s in order to minimize environmental effects. If
the time to fracture is greater than 20 s, use a faster displacement rate than those given in 8.2.4.
8.2.6 Measure the ambient temperature during the test series.
8.2.7 Measure the ambient relative humidity during the test series if tests are performed in laboratory
ambient conditions.
The flexure specimen may be tested with either the wide or narrow face on the loading bearings.
The precrack shall be on the tension surface which is the bottom surface in this figure.
Figure 8 — The flexural specimens on the loading bearings
8.3 Crack size measurement
8.3.1 Examine the fracture surface of the specimens and measure the critical crack dimensions a and 2c as
shown in Figure 4 or 5. Fractographic techniques and fractographic skill are needed for this step. 8.3.2 to
8.3.10 give more detail on the procedures that may be used. Annex B provides guidance on crack detection
and characterization. If stable crack extension is not detected, the critical crack size should be the same as
the precrack size. Measure the crack depth, a, to within 0,005 mm (5 µm) or less if possible and the crack
width, 2c, to within 0,010 mm (10 µm) or less if possible.
NOTE The achievable precision of the crack size measurement depends upon the material and its microstructure, the
clarity of the crack and the mode of viewing. For some materials, it is possible to measure the crack size with greater
precision than suggested in 8.3.1, but in other materials the achievable precision may be less than suggested in 8.3.1. In
many instances, the computed fracture toughness is not very sensitive to the precision of the crack size measurement as
discussed in References [3] and [5]. Depending upon the crack sizes and specimen geometries, satisfactory estimates of
fracture toughness may be obtained even with crack size measurements that are less precise than suggested in 8.3.1.
8.3.2 The optimum procedure will vary from material to material. Either an optical microscope or a scanning
electron microscope, or both may be used. Low magnifications (50× to 100×) may be used to locate the crack,
and higher magnifications (100× to 500×) to directly measure or photograph the crack for measurement.
8.3.3 If an optical microscope is used, then variation of the lighting source direction can be used to highlight
the crack. Stereo binocular optical microscopes are preferred to metallographic microscopes. Crack sizes may
be measured from photos taken of the fracture surface, by direct measurement while viewing the specimen if
the microscope has a precision transversing stage for the specimen, or by an eyepiece filar measurement
device. If photos are taken, the fracture surface plane should be normal to the camera axis and a stage
micrometer should be used to confirm the magnifications.
12 © ISO 2003 — All rights reserved
8.3.4 If a scanning electron microscope (SEM) is used, then an SEM magnification calibration standard
shall be used to confirm the magnification.
NOTE Additional details on techniques to find and characterize the cracks for both optical and SEM microscopy are
given in Annex B.
8.3.5 The crack shape may be approximated by a semi-ellipse. This approximation is most accurate for
instances where the greatest stress intensity factor coefficient is at the deepest part of the crack (Y = Y ;
max d
see 9.1). If the maximum stress intensity factor coefficient is at the surface (Y = Y ), then re-examine the
max s
crack shape to confirm that the crack is semi-elliptical. If it is not, then reject the datum.
8.3.6 If the crack form is severely distorted in the third dimension (i.e. is not flat), or the crack front line is
incomplete over more than 33 % of its periphery, reject the datum. See Figures B.7 c), B.7 e) and B.7 f).
8.3.7 If hand grinding or machining damage [see Figure B.7 a)] interfere with the determination of the crack
shape and Y > Y , then reject the datum.
s d
8.3.8 If the precrack shows evidence of excessive extension (corner pop-in) at the intersection of the
surface [see Figure B.7 b)], then reject the datum.
8.3.9 If the precrack shows evidence of stable crack extension prior to fracture, then measure both the
initial precrack size and the critical crack size. [See Figures B.4 and B.7 d)].
8.3.10 If the crack width is such that 2c > 0,5B or the depth is such that a > 0,5W, then reject the datum. A
smaller indentation load may be used.
8.4 Environmental effects
8.4.1 If susceptibility to environmental degradation, such as slow crack growth, is a concern, then tests
should be performed in accordance with either 8.4.2, 8.4.3 or 8.4.4.
8.4.2 Perform tests at two different displacement rates. The two test rates should differ by at least two or
three orders of magnitude. One rate should be very slow, so that the crack has a chance to react to the
environment. Susceptibility may be evaluated by comparing the mean fracture toughness values at the two
rates. Environmental susceptibility may also be determined by examining the fracture surfaces for evidence of
crack extension such as halos at the slower testing rate [Figures B.4 and B.7 d)]. If the material is susceptible
to environmental effects, then determination of the critical crack size is required. Annex A provides some
examples of the use of the critical crack sizes and also variations of displacement rate. If the precrack size or
incorrect critical crack size is used for the calculation, the fracture toughness values may strongly depend on
the displacement rate.
8.4.3 Perform tests in an inert environment such as dry nitrogen gas. Select an atmosphere which is
considered not to adversely affect the crack growth of the specimen during the flexure test. Recommended
atmospheres include dry air, nitrogen or argon with a purity of 99,9 % or better at atmospheric pressure, or a
vacuum of less than 0,13 Pa. Alternatively, specimens may be coated with a paraffin wax. Use a displacement
rate of 0,5 mm/min.
NOTE 1 For inert atmosphere testing, a simple chamber around the test fixtures or even a sealed plastic bag may be
adequate, provided that the laboratory ambient air can be flushed for several minutes between tests.
NOTE 2 If paraffin wax is used, then avoid contamination of the fracture surface and the precrack after fracture.
8.4.4 Perform one set of experiments in normal laboratory ambient conditions (8.2.2, 8.2.3, and 8.2.4) and
one set of experiments in an inert atmosphere (8.4.3). Environmental susceptibility may be determined by
comparing the mean fracture toughness for the two data sets. Environmental susceptibility may also be
determined by comparing the fracture surfaces and determining whether the laboratory ambient tested
specimens show evidence of crack extension. If environmental sensitivity is detected, use the results from the
inert experiments to compute the fracture toughness. The normal laboratory ambient results may also be used
if the critical crack size is detected.
8.4.5 Fracture toughness, K , should be the fracture toughness for which environmental effects are
Isc
eliminated or minimized. If slow crack growth susceptibility is detected, then report the fracture toughness
determined in inert atmosphere, or the fracture toughness at the fastest loading rates and whenever possible,
the fracture toughness based upon the critical crack size.
8.5 Optional: Estimate of R-curve behaviour
An estimate of the effect of crack size upon fracture toughness (for an assessment of possible R-curve
effects) may be obtained by any one of several methods described in Annex C.
8.6 Optional: Reference materials
Reference materials may be used to verify the procedures in this test method.
9 Calculation
9.1 Calculate the stress intensity shape factor coefficients for both the deepest point of the crack periphery,
Y , and for the surface, Y . Use the critical crack size dimensions.
d s
NOTE The stress intensity factors are from Reference [8] and are only strictly valid for a/c u 1, a/W < 1,0 and
2c/B < 0,5. They may be used for a/c ratios slightly greater than 1 with a slight loss of accuracy according to Reference [9].
For most practical cases, the precracks are much smaller than the cross section dimensions B or W.
For the deepest point of the crack front line:
YM=π()H/Q (2)
d2
where
1,65
Qa=+1 1,464( /c)
Ma=−1,13 0,09( /c)
−1
+−0,54+ 0,89×0,2+ (ac/ ) (a /W )
{}
−1
24 4
+−0,50,65+(ac/) +14×(1−a/)c (a/W)
{}
Ha=−11,22+0,12(/c)(a/W)
0,75 1,5 2
+−0,55 1,05(/ac) +(a/c) (/a W)
For the point at the surface of the crack front line:
YM=π()SH/Q (3)
s1
where
H=−10,34+0,11(ac/)(a/W)
Sa=+1,1 0, 35( /W ) (a /c)
−3 −6 −6
EXAMPLE For W = 3 mm (3 × 10 m), a = 50 × 10 m, and 2c = 120 × 10 m, a/c = 0,833, a/W = 0,017,
Y = 1,267 and Y = 1,292.
d s
14 © ISO 2003 — All rights reserved
9.2 Use the greater value of Y or Y for Y and then compute the fracture toughness, K :
d s max Isc
K =YP3/ABW a (4)
Isc max
where
K is the fracture toughness in megapascals by square root of a metre or meganewtons per metre to
Isc
the power of 3/2;
Y is the maximum stress intensity factor coefficient;
max
A is the four-point fixture moment arm in millimetres, A = (S − S )/2;
o i
P is the break load in newtons;
B is the specimen width in millimetres;
W is the specimen depth in millimetres;
a is the crack depth in metres;
c is the crack half width in metres;
S is the outer (support) span in millimetres;
o
S is the inner (loading) span in millimetres.
i
NOTE The term in parentheses is the flexure strength of the precracked beam in megapascals. It is often useful to
compare this value with the flexural strength of specimens without a precrack, in which fracture occurs from the natural
fracture sources in the material.
9.3 If the specimens are chamfered, and if the chamfer sizes are larger than 0,15 mm, then fracture
toughness values shall be corrected in accordance with Annex D.
9.4 If there is evidence of stable crack extension (8.3.7), then compute the fracture toughness, using
Equation (4) and the critical crack size.
10 Test report
The test report shall include the following information:
a) specimen identification;
b) form of product tested (e.g. sintered, hot-pressed) if data are available;
c) crack plane orientation if available;
d) environment of test, relative humidity, temperature;
e) specimen dimensions B and W;
f) crack dimensions, a and 2c; a statement whether the maximum Y value was at the surface or at the
deepest point of the crack periphery; a general description of the crack. If there is any evidence of stable
crack extension, this evidence shall be reported as well as the initial precrack size and the critical crack
size;
g) fractographic equipment (optical or SEM) used and the approximate magnifications used to observe and
measure the crack;
h) method used to remove the indentation and residual stresses;
i) displacement rate;
j) number of valid test results;
k) individual fracture toughness values, K ;
Isc
l) mean fracture toughness and the standard deviation;
m) whether there is evidence of stable crack extension. If yes, then a report of the fracture toughness based
upon the critical crack size as well as the appar
...
NORME ISO
INTERNATIONALE 18756
Première édition
2003-12-01
Céramiques techniques — Détermination
de la ténacité à la rupture des céramiques
monolithiques à température ambiante
par fissuration superficielle en flexion
Fine ceramics (advanced ceramics, advanced technical ceramics) —
Determination of fracture toughness of monolithic ceramics at room
temperature by the surface crack in flexure (SCF) method
Numéro de référence
©
ISO 2003
PDF – Exonération de responsabilité
Le présent fichier PDF peut contenir des polices de caractères intégrées. Conformément aux conditions de licence d'Adobe, ce fichier
peut être imprimé ou visualisé, mais ne doit pas être modifié à moins que l'ordinateur employé à cet effet ne bénéficie d'une licence
autorisant l'utilisation de ces polices et que celles-ci y soient installées. Lors du téléchargement de ce fichier, les parties concernées
acceptent de fait la responsabilité de ne pas enfreindre les conditions de licence d'Adobe. Le Secrétariat central de l'ISO décline toute
responsabilité en la matière.
Adobe est une marque déposée d'Adobe Systems Incorporated.
Les détails relatifs aux produits logiciels utilisés pour la création du présent fichier PDF sont disponibles dans la rubrique General Info
du fichier; les paramètres de création PDF ont été optimisés pour l'impression. Toutes les mesures ont été prises pour garantir
l'exploitation de ce fichier par les comités membres de l'ISO. Dans le cas peu probable où surviendrait un problème d'utilisation,
veuillez en informer le Secrétariat central à l'adresse donnée ci-dessous.
© ISO 2003
Droits de reproduction réservés. Sauf prescription différente, aucune partie de cette publication ne peut être reproduite ni utilisée sous
quelque forme que ce soit et par aucun procédé, électronique ou mécanique, y compris la photocopie et les microfilms, sans l'accord écrit
de l'ISO à l'adresse ci-après ou du comité membre de l'ISO dans le pays du demandeur.
ISO copyright office
Case postale 56 • CH-1211 Geneva 20
Tel. + 41 22 749 01 11
Fax. + 41 22 749 09 47
E-mail copyright@iso.org
Web www.iso.org
Version française parue en 2005
Publié en Suisse
ii © ISO 2003 – Tous droits réservés
Sommaire Page
Avant-propos .iv
1 Domaine d'application .1
2 Références normatives.1
3 Termes et définitions .2
4 Symboles.3
5 Principe .4
6 Appareillage.5
7 Éprouvettes.6
7.1 Dimensions de l’éprouvette, préparation de l’éprouvette et chanfreinage des arêtes.6
7.2 Nombre d’éprouvettes .6
8 Mode opératoire.7
8.1 Introduction de la préfissure par empreinte Knoop .7
8.2 Rupture de l’éprouvette .11
8.3 Mesurage des dimensions de la fissure .12
8.4 Effets dus au milieu ambiant.13
8.5 Option: estimation du comportement de courbe R .14
8.6 Option: matériaux de référence .14
9 Calcul.14
10 Rapport d’essai.16
Annexe A (informative) Effets dus au milieu ambiant.17
Annexe B (normative) Caractérisation de la préfissure.18
Annexe C (informative) Estimation de la courbe R par la méthode SCF .25
Annexe D (normative) Facteurs de correction du chanfrein.28
Bibliographie.30
Avant-propos
L'ISO (Organisation internationale de normalisation) est une fédération mondiale d'organismes nationaux de
normalisation (comités membres de l'ISO). L'élaboration des Normes internationales est en général confiée
aux comités techniques de l'ISO. Chaque comité membre intéressé par une étude a le droit de faire partie du
comité technique créé à cet effet. Les organisations internationales, gouvernementales et non
gouvernementales, en liaison avec l'ISO participent également aux travaux. L'ISO collabore étroitement avec
la Commission électrotechnique internationale (CEI) en ce qui concerne la normalisation électrotechnique.
Les Normes internationales sont rédigées conformément aux règles données dans les Directives ISO/CEI,
Partie 2.
La tâche principale des comités techniques est d'élaborer les Normes internationales. Les projets de Normes
internationales adoptés par les comités techniques sont soumis aux comités membres pour vote. Leur
publication comme Normes internationales requiert l'approbation de 75 % au moins des comités membres
votants.
L'attention est appelée sur le fait que certains des éléments du présent document peuvent faire l'objet de
droits de propriété intellectuelle ou de droits analogues. L'ISO ne saurait être tenue pour responsable de ne
pas avoir identifié de tels droits de propriété et averti de leur existence.
L'ISO 18756 a été élaborée par le comité technique ISO/TC 206, Céramiques techniques.
iv © ISO 2003 – Tous droits réservés
NORME INTERNATIONALE ISO 18756:2003(F)
Céramiques techniques — Détermination de la ténacité à la
rupture des céramiques monolithiques à température ambiante
par fissuration superficielle en flexion
1 Domaine d'application
La présente Norme internationale décrit une méthode d’essai qui couvre la détermination de la ténacité à la
rupture de matériaux céramiques monolithiques, à température ambiante, par la méthode de fissuration
superficielle en flexion (SCF).
La présente Norme internationale est destinée à être utilisée avec des céramiques monolithiques et des
céramiques à renfort de trichite ou de particules qui sont considérées comme homogènes d’un point de vue
macroscopique. Elle ne couvre pas les composites céramiques à renfort de fibres continues.
La méthode d’essai est applicable aux matériaux ayant des courbes plates ou montantes de résistance à la
propagation de la fissure. Cette méthode est similaire à celle de l’ISO 15732, à l’exception du fait que les
préfissures sont plus petites et sont obtenues par un mode opératoire différent. Il convient que les méthodes
produisent des résultats similaires ou identiques pour les matériaux ayant une courbe R plate.
NOTE Cette méthode d’essai est normalement applicable aux matériaux céramiques ayant une ténacité à la rupture
1/2
inférieure à ≈ 10 MPa·m . Il peut s’avérer difficile de créer des préfissures avec un pénétrateur Knoop pour les matériaux
ayant une ténacité à la rupture supérieure et pour les matériaux mous (faible dureté) comme certaines zircones, ou pour
les céramiques poreuses.
2 Références normatives
Les documents de référence suivants sont indispensables pour l'application du présent document. Pour les
références datées, seule l'édition citée s'applique. Pour les références non datées, la dernière édition du
document de référence s'applique (y compris les éventuels amendements).
ISO 3611:1978, Micromètres d'extérieur
ISO 7500-1:2004, Matériaux métalliques — Vérification des machines pour essais statiques uniaxiaux —
Partie 1: Machines d'essai de traction/compression — Vérification et étalonnage du système de mesure de
force
ISO 14704:2000, Céramiques techniques — Méthode d'essai de résistance en flexion des céramiques
monolithiques à température ambiante
3 Termes et définitions
Pour les besoins du présent document, les termes et définitions suivants s’appliquent.
3.1
facteur d’intensité de contrainte
K
l
grandeur du champ de contrainte élastique à l'extrémité de la fissure soumise à un chargement en mode
d'ouverture
NOTE Il est fonction de la force appliquée, des dimensions et de la forme de l'éprouvette, ainsi que de la longueur de
la fissure, et a les dimensions d'une force multipliée par une longueur à la puissance 3/2.
3.2
ténacité à la rupture
terme générique pour les mesures de résistance à la propagation d’une fissure
3.3
valeur de ténacité à la rupture
K
lsc
valeur de ténacité à la rupture mesurée par la méthode SCF
NOTE Il s’agit du facteur d’intensité de contrainte mesuré correspondant à la résistance à la propagation d’une petite
fissure semi-elliptique formée sous une empreinte Knoop. Le mesurage est effectué selon le présent mode opératoire et
satisfait à toutes les conditions de validité.
3.4
préfissure
fissure introduite artificiellement dans une éprouvette avant de soumettre l’éprouvette à un essai de rupture
3.5
front de la fissure
ligne indiquant la position de l’extrémité de la fissure
3.6
facteur critique d’intensité de contrainte
K
lc
valeur critique de K à laquelle se produit la rupture rapide
l
3.7
fissure critique
fissure à la rupture à une charge maximale et dont le facteur d’intensité de contrainte atteint tout juste le
facteur critique d’intensité de contrainte
3.8
dimensions de la fissure critique
dimensions de la fissure critique à la rupture
NOTE La fissure critique sera de dimensions plus importantes que la préfissure si une propagation stable de la
fissure se produit en raison d’un accroissement lent de la fissure favorisé par le milieu ambiant ou d’une courbe R
montante.
3.9
flexion quatre points 1/4 de point
configuration spécifique d'essai de résistance en flexion quatre points dans laquelle les cylindres intérieurs
sont décalés d'un quart de la portée d'appui par rapport aux deux cylindres extérieurs
2 © ISO 2003 – Tous droits réservés
3.10
flexion quatre point 1/3 de point
configuration spécifique d'essai de résistance en flexion quatre points dans laquelle les cylindres intérieurs
sont décalés d'un tiers de la portée d'appui par rapport aux deux cylindres extérieurs
3.11
résistance en flexion
contrainte nominale maximale supportée par une éprouvette élastique spécifiée lors d'un essai de flexion
conduit jusqu'à rupture
4 Symboles
a Profondeur de la fissure
A Bras de levier du dispositif de flexion
B Largeur de l’éprouvette, dimension de la section transversale perpendiculaire à la direction du
chargement en flexion
c Demi-largeur de la fissure
C Dimensions du chanfrein
d Longueur de la longue diagonale de l’empreinte Knoop
h Profondeur de l’empreinte Knoop
F Charge d’empreinte Knoop
F Facteur de correction du chanfrein
c
H (a/c, a/W) Fonction polynomiale dans le coefficient du facteur d’intensité de contrainte, relative au point où, à
la périphérie de la fissure, cette dernière coupe la surface de l’éprouvette
H (a/c, a/W) Fonction polynomiale dans le coefficient du facteur d’intensité de contrainte, relative à la partie la
plus profonde de la fissure superficielle
K Facteur d’intensité de contrainte, Mode I
l
K Facteur critique d’intensité de contrainte, Mode I
lc
K Valeur de la ténacité à la rupture, méthode de fissuration superficielle en flexion
lsc
L Portée d’appui du dispositif de flexion
L Longueur de l’éprouvette
T
M (a/c, a/W) Fonction polynomiale dans le coefficient du facteur d’intensité de contrainte
P Charge à la rupture
Q (a/c) Fonction polynomiale de l’ellipticité de la fissure superficielle
S (a/c, a/W) Facteur dans le coefficient du facteur d’intensité de contrainte
W Profondeur de l’éprouvette, dimension de la section transversale qui est parallèle à la direction de
chargement en flexion
Y Coefficient du facteur d’intensité de contrainte
Y Coefficient du facteur d’intensité de contrainte au niveau de la partie la plus profonde de la fissure
d
superficielle
Y Coefficient maximal du facteur d’intensité de contrainte le long de la frontière de la fissure
max
superficielle
Y Coefficient du facteur d’intensité de contrainte à l’intersection de la fissure superficielle avec la
s
surface de l’éprouvette
5 Principe
La présente Norme internationale est applicable au développement et à la comparaison de matériaux, à
l'assurance qualité, à la caractérisation, à la fiabilité et à la génération de données de fabrication. La méthode
détermine la valeur de ténacité à la rupture, K , en rompant une éprouvette de flexion courante ayant une
lsc
petite préfissure superficielle (voir la Figure 1). L’éprouvette est poinçonnée avec un pénétrateur Knoop afin
de créer une petite fissure superficielle semi-elliptique. L’éprouvette est polie ou meulée soigneusement
jusqu’à ce que l’empreinte et le champ de contraintes résiduelles associé soient éliminés. L’éprouvette est
rompue en flexion quatre points. La ténacité à la rupture, K , est calculée à partir de la charge de rupture et
lsc
des dimensions mesurées de la fissure critique. Il est nécessaire d’avoir recours à la fractographie pour
mesurer les dimensions de la préfissure et déterminer si les dimensions de la fissure ont augmenté. La
ténacité à la rupture en fonction des dimensions de la fissure peut être évaluée en faisant varier la charge
d’empreinte utilisée pour créer la préfissure. Des informations concernant cette méthode d’essai peuvent être
obtenues dans les Références [1] et [2]. Un projet d’étude comparative interlaboratoires internationale sur
cette méthode est décrit dans les Références [3],[4] et [5].
Légende
1 empreinte et préfissure
2 surface polie ou rodée
Figure 1 — Empreinte et préfissure dans une éprouvette en flexion
Si le matériau céramique est trop mou (faible dureté) ou a une ténacité à la rupture trop importante, il peut
s’avérer difficile de créer une préfissure par la méthode SCF. De plus, pour certains matériaux (en particulier
ceux à gros grains ou à microstructures hétérogènes), il peut s’avérer difficile de détecter la fissure sur la
surface de rupture. Si l’utilisateur n’est pas certain de l’applicabilité de cette méthode, une seule éprouvette
d’épreuve peut alors être mise à l’essai suivant un mode opératoire abrégé. Réaliser une empreinte sur
l’éprouvette et la rompre sans enlever l’empreinte et les contraintes résiduelles. Inspecter la surface de
rupture pour confirmer que l’éprouvette s’est rompue à partir de la préfissure (et non à partir d’un défaut du
matériau) et que la préfissure peut être détectée sur la surface de rupture.
4 © ISO 2003 – Tous droits réservés
Dans la présente Norme internationale, la préfissuration est réalisée par empreinte Knoop uniquement. Dans
cette méthode d’essai, les contraintes résiduelles sous l’empreinte sont éliminées. On dispose d’une
[3][4][5][6][7]
expérience limitée de la préfissuration SCF par empreinte Vickers .
6 Appareillage
6.1 Une machine d’essai, capable d’appliquer une vitesse de traverse uniforme. La machine d’essai doit
être conforme à l’ISO 7500-1:2004, Classe 1, avec une exactitude de 1 % de la charge indiquée à la rupture.
6.2 Un dispositif de flexion, quatre points tel qu’illustré à la Figure 2. Le dispositif de flexion doit satisfaire
aux exigences de l’ISO 14704.
Le dispositif doit être soit semi-articulé, soit entièrement articulé, en fonction de l’état des éprouvettes. Si les
éprouvettes répondent aux exigences de parallélisme de 7.1, alors un dispositif semi-articulé peut être utilisé.
Un dispositif semi-articulé est en général entièrement satisfaisant pour des éprouvettes usinées. Si les
éprouvettes ne satisfont pas aux exigences de parallélisme de 7.1 (en raison d’inégalités du meulage manuel,
de problèmes d’usinage ou d’autres causes), un dispositif entièrement articulé doit être utilisé. Un dispositif
entièrement articulé peut également être utilisé avec des éprouvettes usinées. Les éprouvettes doivent être
chargées et maintenues par des cylindres. Les cylindres doivent être libres en rotation afin d’éliminer le
frottement. Pour la flexion quatre points, les deux cylindres intérieurs doivent être libres de rouler vers
l’intérieur, et les deux cylindres extérieurs doivent être libres de rouler vers l’extérieur.
Un dispositif quatre points 1/4 de point avec 20 mm de portée d’appui et 10 mm de portée intérieure est
également autorisé. Un tel dispositif doit satisfaire aux exigences de l’ISO 14704.
Dimensions en millimètres
L = 40,0 ± 0,10, ou L = 20,0 ± 0,10
a) Flexion quatre points 1/4 de point
L = 30,0 ± 0,10
b) Flexion quatre points 1/3 de point
Légende
1 cylindres de chargement
2 cylindres de support
Figure 2 — Flexion quatre points
6.3 Un micromètre, tel que décrit dans l’ISO 3611, mais avec une résolution de 0,002 mm, doit être utilisé
pour mesurer les dimensions de l’éprouvette. Les faces de touche fixe du micromètre doivent être planes
comme indiqué dans l'ISO 3611. Le micromètre ne doit pas avoir d'extrémité sphérique ou acérée qui pourrait
endommager l'éprouvette. D'autres instruments de mesure de dimensions peuvent être utilisés s'ils ont au
moins une résolution de 0,002 mm.
6.4 Une machine d’essai de dureté, du type conventionnel, pour créer l’empreinte Knoop. La machine
doit pouvoir appliquer des charges de 20 N à 50 N ou supérieures. Si une machine d’essai de dureté avec
cette fourchette de charge n’est pas disponible, une machine d’essai de résistance (6.1) peut être utilisée,
bien qu’il puisse en résulter une certaine perte de précision ou de maîtrise de l’empreinte et des dimensions
de la fissure.
6.5 Des microscopes, optique et/ou électronique à balayage, doivent être utilisés pour détecter la
préfissure (ou la fissure critique) et mesurer ses dimensions sur la surface de rupture de l’éprouvette après
l’essai. Des grossissements de 100 × ou 500 × sont en général exigés. Le microscope doit pouvoir réaliser
des enregistrements photographiques ou numériques des fissures.
6.6 Des colorants pénétrants, pour mettre en évidence la fissure. Les colorants pénétrants qui ne
favorisent pas l’accroissement lent de la fissure et ne migrent pas (c'est-à-dire ne se répandent pas sur la
surface de rupture après la rupture) sont préférés.
6.7 Un dispositif de mesure de la température, un thermomètre ou un autre dispositif, pour mesurer la
température ambiante lors de la rupture de l’éprouvette.
6.8 Un dispositif de mesure de l’humidité, tel qu’un hygromètre, un psychromètre fronde ou un autre
dispositif, pour mesurer l’humidité ambiante lors de la rupture de l’éprouvette.
7 Éprouvettes
7.1 Dimensions de l’éprouvette, préparation de l’éprouvette et chanfreinage des arêtes
7.11 Des éprouvettes rectangulaires de dimensions telles qu’indiquées à la Figure 3 doivent être utilisées.
Les tolérances de section transversale sont de ± 0,2 mm. La tolérance de parallélisme sur les faces
longitudinales opposées est de 0,015 mm.
7.1.2 Les éprouvettes doivent être préparées conformément à l’ISO 14704, avec les exceptions notées
ci-après. L’empreinte peut être réalisée dans une face de 3 mm de largeur ou dans une face de 4 mm de
largeur. Une meule diamantée de grain 320 au maximum doit être utilisé pour éliminer les derniers 0,04 mm
sur la surface qui est utilisée pour l’empreinte. Cette surface doit être polie, rodée ou finement meulée pour
obtenir une surface plane et lisse pour la fissure superficielle.
NOTE La surface n’exige pas une finition de polissage de haute qualité telle que celle qui est exigée pour un
mesurage de dureté. La surface doit simplement être plane de façon que l’empreinte Knoop ne soit pas affectée par les
stries ou les marques d’usinage ou la non-planéité de l’éprouvette.
7.1.3 Le chanfreinage ou l’arrondi des arêtes sont facultatifs. Si une rupture prématurée se produit à partir
de l'endommagement d’une arête, les arêtes doivent être chanfreinées ou arrondies comme cela est spécifié
dans l’ISO 14704. Il convient que les dimensions du chanfrein soient de 0,15 mm ou moins. Voir la Figure 3.
7.2 Nombre d’éprouvettes
Le nombre d’éprouvettes ne doit pas être inférieur à cinq. Il est recommandé de préparer au moins dix
éprouvettes. Ceci fournira des éprouvettes pour réaliser des essais préliminaires destinés à déterminer les
meilleures charges d’empreinte et prévoir les éprouvettes de remplacement en cas d’essais non réussis ou
invalides. Davantage d’éprouvettes sont nécessaires s’il est nécessaire de faire varier le milieu ambiant, la
vitesse de l’essai ou les dimensions de la préfissure.
6 © ISO 2003 – Tous droits réservés
Dimensions en millimètres
L W 25 pour dispositif d’essai 20 mm, ou
T
L W 35 pour dispositif d’essai 30 mm, ou
T
L W 45 pour dispositif d’essai 40 mm
T
a
Chanfreins ou arrondis d’arêtes.
Figure 3 — Dimensions de l’éprouvette
8 Mode opératoire
8.1 Introduction de la préfissure par empreinte Knoop
8.1.1 Utiliser un pénétrateur Knoop pour créer une empreinte au milieu de la surface polie, rodée ou
finement meulée de l’éprouvette. L’empreinte doit être perpendiculaire à l’axe longitudinal de l’éprouvette, à 2°
près, comme montré à la Figure 1. Une extrémité de l’éprouvette doit être inclinée de 0,25° à 0,5° environ
comme montré à la Figure 4. Un temps d’empreinte en pleine charge de 15 s ou plus durant le cycle
d’empreinte doit être utilisée. L’empreinte peut être réalisée soit dans une face de 3 mm de largeur, soit dans
une face de 4 mm de largeur, comme illustré à la Figure 5. Il est recommandé de placer l’empreinte près du
centre exact de la surface, par rapport à la dimension de largeur B et à la longueur de l’éprouvette, afin de
pouvoir confirmer facilement que la rupture se produit à partir de la préfissure.
NOTE 1 L’inclinaison de 0,25° à 0,5° facilite la détection de la préfissure sur la surface de rupture. L’inclinaison de
l’éprouvette crée des inclinaisons de la préfissure de 0° à 5°.
NOTE 2 Dans certains cas, avec la zircone par exemple, des temps d’empreinte supérieurs à 15 s peuvent être utiles.
NOTE 3 Une éprouvette d’épreuve peut être mise à l’essai pour aider à déterminer la meilleure charge d’empreinte.
Réaliser l’empreinte, puis rompre l’éprouvette dans le dispositif de flexion sans éliminer l’empreinte et la zone de
dommages dus aux contraintes résiduelles. Examiner la surface de rupture pour confirmer que l’éprouvette s’est rompue à
partir de la préfissure, que la préfissure est discernable et dans les limites dimensionnelles prescrites.
NOTE 4 Le mode opératoire d’empreinte Knoop pour créer une fissure superficielle ne réussira pas sur des
céramiques très molles ou poreuses car une préfissure ne se formera pas par l’empreinte. Il se peut que le processus ne
fonctionne pas sur des céramiques très dures qui sont résistantes à la formation de fissures ou lorsque les fissures sont
très petites et seront probablement éliminées durant l’étape suivante de polissage, destinée à éliminer la zone de
dommages dus aux contraintes résiduelles.
a) Vue latérale de l’éprouvette b) Vue de l’extrémité de l’éprouvette
Légende
1 pénétrateur Knoop
2 préfissure
3 empreinte avec préfissure
4 éprouvette sur plate-forme d’inclinaison
Figure 4 — Empreinte de préfissuration par empreinte Knoop
NOTE 1 L’empreinte peut être située soit sur la face large de 4 mm, soit sur la face étroite de 3 mm.
NOTE 2 Les dimensions de la fissure, exagérées pour l’illustration, sont en général beaucoup plus petites.
Figure 5 — Section transversale de l’éprouvette
8.1.2 Il peut s’avérer nécessaire de déterminer pour chaque classe différente de matériaux la charge
d’empreinte optimale en utilisant quelques éprouvettes d’épreuve. La charge doit être suffisante pour créer
une fissure plus grande que les défauts apparaissant naturellement dans le matériau, mais pas trop grande
par rapport aux dimensions de la section de l’éprouvette (2c < 0,5B et a > 0,5W) et pas grande au point que
l’empreinte s’écaille ou se fissure sérieusement. Des charges d’empreinte d’environ 20 N conviennent aux
céramiques très cassantes, des charges de 25 N à 50 N aux céramiques de dureté moyenne et des charges
de 49 N à 98 N aux céramiques très dures ou ayant une certaine porosité. Des charges d’empreinte de 98 N
à 147 N peuvent être nécessaires pour les matériaux à grains de taille moyenne à grosse. Dans de tels
matériaux, il est nécessaire de créer de grandes préfissures qui se dégageront de la rugosité microstructurale
normale de la surface de rupture.
8 © ISO 2003 – Tous droits réservés
8.1.3 Mesurer la longue diagonale, d, de l’empreinte Knoop à 0,005 mm (5 µm) près.
NOTE Une machine conventionnelle d’essai de la microdureté (6.4) peut être utilisée pour ce mesurage. Le
mesurage n’exige pas la fidélité requise pour les mesurages de la dureté. Si la dureté Knoop est rapportée, un plus grand
soin est recommandé pour le mesurage de la dimension diagonale et la préparation de la surface initiale de l’éprouvette.
8.1.4 Calculer la profondeur, h, de l’empreinte Knoop, comme suit:
hd= /30 (1)
8.1.5 Mesurer la profondeur de l’éprouvette, W, au milieu de l’éprouvette à l’emplacement de l’empreinte, à
0,002 mm près. Un micromètre manuel (6.3) avec les graduations du vernier indiquées par pas de 0,002 mm
est approprié.
8.1.6 Marquer d’une flèche le côté de l’éprouvette avec un crayon ou autre marqueur pour indiquer la
surface sur laquelle est située la préfissure.
8.1.7 Éliminer l’empreinte et la zone de dommages dus aux contraintes résiduelles.
8.1.7.1 Enlever de la face sur laquelle se trouve l’empreinte une quantité de matière sur une épaisseur
de 4,5 h à 5,0 h environ, comme indiqué à la Figure 6. Le processus d’élimination de matière ne doit pas
induire des contraintes résiduelles ou des dommages d’usinage excessifs à la surface de l’éprouvette.
Prendre soin d’enlever la matière sur la bonne face. Marquer avec un crayon ou un marqueur permanent les
faces qui ne seront pas meulées ou polies. La matière peut être enlevée par l’un quelconque des trois modes
opératoires décrits en 8.1.7.2, 8.1.7.3 et 8.1.7.4.
NOTE L’élimination de 4,5 h à 5,0 h de matière supprime la zone de dommages dus aux contraintes résiduelles sous
l’empreinte et, d’ordinaire, laisse une préfissure d’une forme ayant le plus important facteur d’intensité de contrainte à la
partie la plus profonde de la périphérie de la préfissure. L’emplacement de l’intensité maximale de contrainte peut être
contrôlé par la quantité de matière enlevée. La préfissure initiale sous empreinte Knoop est approximativement semi-
circulaire et le coefficient maximal du facteur d’intensité de contrainte, Y , est en surface. À mesure que la matière est
max
enlevée, la préfissure tend à devenir de forme semi-elliptique (ou semblable à une section d’un cercle) et Y se
max
déplacera vers la partie la plus profonde de la préfissure. Si une trop grande quantité de matière est enlevée, la préfissure
restante sera trop petite et la rupture ne se produira pas à partir de la préfissure. Dans de tels cas, il est préférable
d’enlever des quantités plus petites, à la condition qu’une épaisseur de 3 h au minimum soit éliminée. Si cette étape n’est
pas suffisante pour garantir la rupture à partir de la préfissure, alors il se peut qu’une charge d’empreinte plus importante
soit nécessaire.
Légende
1 matière à éliminer après empreinte
NOTE La préfissure s’étend au-dessous de l’empreinte de dureté Knoop, qui a une profondeur h.
Figure 6 — L'empreinte et la zone de dommages dus aux contraintes résiduelles
8.1.7.2 La matière peut être éliminée par meulage manuel, rodage manuel ou polissage manuel avec un
papier abrasif en conditions humides ou sèches. Pour de nombreuses céramiques, le polissage manuel de
l’éprouvette avec un papier au carbure de silicium de grain 180 à 220 peut éliminer la quantité requise en
5 min à 10 min par éprouvette. Vérifier fréquemment la hauteur de l’éprouvette durant ce processus. Éliminer
les derniers 0,005 mm avec un papier de grain plus fin (220 à 280) en imprimant une pression moindre, de
façon à réduire au minimum les dommages dus au polissage. Surveiller fréquemment la profondeur de
l’éprouvette, W, durant l’étape de l’élimination de matière, en surveillant tout particulièrement l’uniformité de
cette élimination.
Il se peut que le meulage, le rodage ou le polissage manuels ne soient pas efficaces pour les céramiques très
dures. Dans ce cas, la matière peut être enlevée par un polissage ou un rodage à la machine (8.1.7.3), ou par
un meulage de la surface à la machine (8.1.7.4).
Changer régulièrement l’orientation de la surface polie ou meulée manuellement durant l’élimination de
matière afin de réduire au minimum l’inégalité de la surface. Cette dernière peut causer des défauts
d’alignement durant les essais de flexion subséquents ou causer des erreurs dans les mesures des
dimensions de la section transversale.
NOTE 1 Le meulage manuel à sec peut être plus rapide que le meulage en conditions humides. Des disques de
polissage imprégnés de diamants (30 µm) sont également efficaces pour éliminer la matière par meulage manuel.
NOTE 2 Le rodage ou le meulage manuels peuvent créer une inégalité de la surface préfissurée ou son défaut de
parallélisme par rapport à la surface opposée de l’éprouvette. Un léger arrondi des bords de l’éprouvette ne porte en
général pas à conséquence.
NOTE 3 Des papiers à grain plus fin (320 à 500) sont recommandés pour les verres, à la fois pour l’élimination
grossière de matière et la finition.
AVERTISSEMENT — Des poudres céramiques fines ou des fragments fins peuvent être créés si le
rodage ou le sablage manuels sont effectués à sec. Il convient de porter des masques ou de réaliser
l’élimination en conditions humides s’il y a un risque d’inhalation, en particulier si la céramique
contient de la silice ou des trichites fines.
8.1.7.3 La matière peut être enlevée par polissage ou rodage à la machine avec une pâte de diamant
contenant des particules d’environ 0,3 µm. Pour de nombreuses céramiques, cette opération demande
environ 10 min à 15 min par éprouvette. Une éprouvette d’épreuve peut être polie pour obtenir un taux
d’élimination de matière approprié en réglant les masses appliquées, la vitesse de rotation du disque et les
durées de polissage afin d’obtenir la quantité appropriée de matière enlevée.
8.1.7.4 La matière peut être enlevée par un meulage de surface avec des meules diamantées fixées sur
une machine à meuler pour matériaux très durs. S’assurer que la quantité appropriée de matière a été
enlevée de chaque éprouvette. Éviter des conditions de meulage forcé qui peuvent introduire des contraintes
résiduelles. Si le meulage de la surface à la machine est utilisé, une meule à grain fin (320 à 600) et de petits
taux d’élimination sont recommandés. Le meulage peut être effectué en conditions humides.
8.1.7.5 Après que la quantité de matière prescrite a été enlevée, examiner la surface meulée et portant
l’empreinte pour établir s’il subsiste des fissures latérales. La Figure 7 donne des indications. Un microscope
optique à faible puissance et à lumière réfléchie pour usage métallurgique (6.5) avec des grossissements
de 100 × à 500 × peut être utilisé pour examiner la surface en traction meulée et portant l’empreinte. Si l’on
n’observe pas de fissures latérales subsistantes, il convient alors d’enlever plus de matière (6 h à 10 h) pour
s’assurer que les fissures latérales restantes sont éliminées.
NOTE Des fissures latérales plus profondes que la normale peuvent se produire dans les matériaux ayant une très
1/2
faible ténacité à la rupture (< 3,0 MPa·m ) ou si des charges d’empreinte plus importantes (W 98 N) sont utilisées.
10 © ISO 2003 – Tous droits réservés
a) montre la surface meulée après l’élimination de matière. L’empreinte Knoop (lignes pointillées) a été éliminée et
la fissure médiane est très étroite et non visible. Il n’y a pas de traces de fissures latérales.
b) à e) montrent des exemples de fissures latérales subsistantes qu’il convient d’éliminer conformément à 8.1.7.4
et 8.1.7.5.
Figure 7 — Surface meulée et fissures latérales subsistant après l’élimination de la zone endommagée
dans certains matériaux cassants
8.1.7.6 Le recuit ou le traitement thermique pour éliminer les contraintes résiduelles sous l’empreinte ne
sont pas autorisés par la présente Norme internationale en raison du risque que la tête de la fissure ne
s’émousse ou que la fissure ne se cicatrise.
8.1.8 Sécher l’éprouvette avant l’essai si l’élimination de matière est réalisée en conditions humides.
NOTE Il n’existe pas de consensus sur les meilleures conditions pour sécher les éprouvettes. Le séchage dans une
étuve à air ou à vide à une température de 100 °C à 150 °C et sur une durée allant jusqu’à 1 h, puis le stockage dans un
dessiccateur avant l’essai, peut s’avérer suffisant.
8.1.9 Si nécessaire, un colorant pénétrant (6.6) peut être appliqué pour aider à détecter la fissure. Si un
colorant pénétrant est utilisé, il convient que l’éprouvette soit séchée intégralement avant la rupture.
8.1.10 Mesurer et enregistrer les dimensions de l’éprouvette, B et W, dans le voisinage de la préfissure.
à 0,002 mm près.
8.2 Rupture de l’éprouvette
8.2.1 S’assurer que l’éprouvette est sèche.
8.2.2 Soumettre les éprouvettes préfissurées à un essai de flexion quatre points jusqu’à la rupture dans des
conditions ambiantes de laboratoire. Si le matériau a une propension à un accroissement lent de la fissure, il
est recommandé d’appliquer les conditions d’essai de 8.4.
NOTE De nombreux oxydes, verres et céramiques ayant une phase vitreuse peuvent être susceptibles d’un
accroissement lent de la fissure. La ténacité à la rupture mesurée peut être sensible à la vitesse de déplacement et à
l’humidité ambiante. Voir l’Annexe A pour des informations supplémentaires.
8.2.3 Insérer l’éprouvette dans le dispositif de flexion comme indiqué à la Figure 8, la fissure superficielle
étant sur la face en traction, approximativement au milieu (à 1 mm près) des deux cylindres de chargement
intérieurs. L’éprouvette peut être préchargée à 25 % au maximum de la charge de rupture escomptée. Mettre
du coton, du tissu chiffonné ou un autre matériau approprié sous l’éprouvette pour empêcher les morceaux de
heurter le dispositif lors de la rupture et prévenir l’endommagement de la surface de rupture par un choc
survenant après la rupture de l’éprouvette. Placer un simple bouclier de protection autour du dispositif pour
garantir la sécurité de l’opérateur et pour conserver les morceaux primaires résultant de la rupture pour une
analyse subséquente de la rupture. Si la face préfissurée de l’éprouvette n’est pas parallèle à la face
opposée, à 0,015 mm près, alors un dispositif à articulation complète doit être utilisé.
8.2.4 Utiliser une vitesse de déplacement normale de 0,5 mm/min pour les éprouvettes mises à l’essai avec
un dispositif dont la portée d’appui est de 30 mm ou 40 mm. Utiliser une vitesse de déplacement
de 0,10 mm/min à 0,13 mm/min pour les éprouvettes mises à l’essai avec un dispositif dont la portée d’appui
est de 20 mm.
8.2.5 Appliquer une charge de compression au dispositif jusqu’à ce que l’éprouvette se rompe. Mesurer la
charge en rupture avec une exactitude de ± 1 %. Il convient que le temps jusqu’à la rupture ne dépasse
pas 20 s afin de réduire au minimum les effets dus au milieu ambiant. Si le temps jusqu’à la rupture est
supérieur à 20 s, utiliser une vitesse de déplacement plus rapide que celles indiquées en 8.2.4.
8.2.6 Mesurer la température ambiante durant toute la série d’essai.
8.2.7 Mesurer l’humidité relative ambiante durant toute la série d’essai si les essais sont réalisés dans des
conditions ambiantes de laboratoire.
L’éprouvette de flexion peut être mise à l’essai avec soit la face large, soit la face étroite sur les cylindres de chargement.
La préfissure doit être située sur la surface en traction qui, sur cette figure, est la surface du bas.
Figure 8 — Éprouvettes en flexion sur les cylindres de chargement
8.3 Mesurage des dimensions de la fissure
8.3.1 Examiner la surface de rupture sur les éprouvettes et mesurer les dimensions de la fissure critique a
et 2c comme indiqué à la Figure 4 ou à la Figure 5. Des techniques fractographiques et des compétences en
fractographie sont nécessaires à cette étape. Les Paragraphes 8.3.2 à 8.3.10 donnent plus de précisions sur
les modes opératoires utilisables. L’Annexe B fournit des indications sur la détection et la caractérisation des
fissures. Si une propagation stable de la fissure n’est pas détectée, il convient que les dimensions de la
fissure critique soient identiques aux dimensions de la préfissure. Mesurer la profondeur de la fissure, a, à
0,005 mm (5 µm) près ou moins si possible, et la largeur de la fissure, 2c, à 0,010 mm (10 µms) près ou
moins si possible.
12 © ISO 2003 – Tous droits réservés
NOTE La précision réalisable du mesurage des dimensions de la fissure dépend du matériau et de sa
microstructure, de la netteté de la fissure et du mode de visualisation. Pour certains matériaux, il est possible de mesurer
les dimensions de la fissure avec une plus grande précision que cela n’est suggéré en 8.3.1, mais, dans le cas d’autres
matériaux, la précision réalisable peut être inférieure à ce qui est suggéré en 8.3.1. Dans de nombreux cas, la ténacité à
la rupture qui est calculée n’est pas très sensible à la précision du mesurage des dimensions de la fissure, comme cela
est examiné dans les Références [3] et [5]. Selon les dimensions de la fissure et les géométries d’éprouvettes, des
estimations satisfaisantes de la ténacité à la rupture peuvent être obtenues même lorsque les mesurages des dimensions
de la fissure sont moins précis que cela n’est suggéré en 8.3.1.
8.3.2 Le mode opératoire optimal variera selon les matériaux. Un microscope optique, un microscope
électronique à balayage, ou les deux, peuvent être utilisés. De faibles grossissements (50 × à 100 ×) peuvent
être utilisés pour localiser la fissure, et des grossissements supérieurs (100 × à 500 ×) peuvent être utilisés
pour mesurer directement ou photographier la fissure pour le mesurage.
8.3.3 Si un microscope optique est utilisé, alors il est possible de faire varier l’orientation de la source
d’éclairage pour mettre en évidence la fissure. Les microscopes optiques stéréo-binoculaires sont préférés
aux microscopes métallographiques. Les dimensions de fissures peuvent être mesurées à partir de
photographies de la surface de rupture, par mesurage direct en visualisant l’éprouvette si le microscope a une
platine à déplacement transversal de précision, ou par un dispositif de mesurage avec oculaire de réglage à
fil. Si des photographies sont prises, il convient que le plan de la surface de rupture soit perpendiculaire à
l’axe de l’appareil photographique et qu’un micromètre de microscope soit utilisé pour confirmer les
grossissements.
8.3.4 Si un microscope électronique à balayage (SEM) est utilisé, alors un étalon du grossissement SEM
doit être utilisé pour confirmer le grossissement.
NOTE Des précisions supplémentaires sur les techniques permettant de localiser et de caractériser les fissures en
microscopie optique et SEM sont données dans l’Annexe B.
8.3.5 La configuration de la fissure peut être approchée par une demi-ellipse. Cette approximation est des
plus précises dans le cas où le plus important coefficient du facteur d’intensité de contrainte est situé au
niveau de la partie la plus profonde de la fissure (Y = Y ; voir 9.1). Si le coefficient maximal du facteur
max d
d’intensité de contrainte est situé à la surface (Y = Y ), réexaminer alors la configuration de la fissure pour
max s
confirmer que la fissure est semi-elliptique. Si tel n’est pas le cas, alors rejeter les données observées.
8.3.6 Si la configuration de la fissure est fortement déformée dans la troisième dimension (c'est-à-dire n’est
pas plate), ou si le front de la fissure est incomplet sur plus de 33 % de la périphérie de la fissure, rejeter les
données. Voir les Figures B.7 c), B.7 e) et B.7 f).
8.3.7 Si des dommages dus au meulage manuels ou à l’usinage [voir la Figure B.7 a)] interférent avec la
détermination de la configuration de la fissure et si Y > Y , alors rejeter les données.
s d
8.3.8 Si la préfissure montre une propagation excessive («fissure subite» du coin) à l’intersection de la
surface [voir la Figure B.7 b)], alors rejeter les données.
8.3.9 Si la préfissure montre une propagation stable de la fissure avant la rupture, alors mesurer à la fois
les dimensions initiales de la préfissure et les dimensions de la fissure critique [voir les Figures B.4 et B.7 d)].
8.3.10 Si la largeur de la fissure est telle que 2c > 0,5B ou si sa profondeur est telle que a > 0,5W, alors
rejeter les données. Une charge d’empreinte plus petite peut être utilisée.
8.4 Effets dus au milieu ambiant
8.4.1 Si la sensibilité à la dégradation du milieu ambiant, donnant lieu par exemple à un accroissement lent
de la fissure, est préoccupante, alors il convient de réaliser des essais conformément à 8.4.2, 8.4.3 ou 8.4.4.
8.4.2 Réaliser des essais à deux vitesses de déplacement différentes. Il convient que les deux vitesses
d’essai diffèrent d’au moins deux ou trois ordres de grandeur. Il convient qu’une vitesse soit très lente, de
sorte que la fissure ait la possibilité de réagir au milieu ambiant. Il est possible d’évaluer la sensibilité au
milieu ambiant en comparant les valeurs moyennes de la ténacité à la rupture aux deux vitesses
...