ISO 17565:2003
(Main)Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for flexural strength of monolithic ceramics at elevated temperature
- Abstract
ISO 17565:2003 describes the method of test for determining the flexural strength of monolithic fine ceramics and whisker- or particulate-reinforced ceramic composites at elevated temperature. Flexural strength is one measure of the uniaxial strength of fine ceramics. This test method may be used for materials development, quality control, characterization and design data generation purposes.
- Status
- Published
- Publication Date
- 11-Dec-2003
- Technical Committee
- ISO/TC 206 - Fine ceramics
- Current Stage
- 9092 - International Standard to be revised - 90 Review
- Start Date
- 20-Oct-2025
Overview
ISO 17565:2003 - "Fine ceramics (advanced ceramics, advanced technical ceramics) - Test method for flexural strength of monolithic ceramics at elevated temperature" - specifies a standardized method to determine the flexural strength of monolithic fine ceramics and whisker- or particulate-reinforced ceramic composites when tested at elevated temperatures. The procedure supports materials development, quality control, mechanical characterization and generation of design data for high-temperature ceramic components.
Key topics and technical requirements
- Test principle: Rectangular beam specimens are loaded in bending (three- or four-point flexure) at elevated temperature until fracture; fracture load and geometry are used to compute flexural strength.
- Test configurations: Three-point, four-point-1/4 and four-point-1/3 flexure are described (four-point-1/4 recommended to expose more material to maximum stress).
- Apparatus:
- Testing machine: Class 1 accuracy (verification per ISO 7500-1) - typically 1% accuracy of indicated load at fracture.
- Heating device/furnace: Maintain uniform and stable specimen temperature (control within ±2 °C; specimen temperature variation limited, and equilibrium time determined).
- Temperature measurement: Use thermocouples per IEC 60584-1 (low thermal inertia, wire diameter ≤ 0.5 mm); instruments with at least 1 °C resolution and appropriate accuracy. Radiation pyrometry may be used with emissivity corrections.
- Testing fixture and bearings: Semi- or fully-articulating three- or four-point fixtures; cylindrical rolling bearings with diameter ≈ 1.5 × specimen thickness (recommended 4.5–5.0 mm), length ≥ 12 mm, uniform to ±0.015 mm to minimize friction and contact errors.
- Specimen preparation & dimensions: Rectangular beam geometry and surface/chamfer considerations are specified; corrections for chamfer size and thermal expansion are included.
- Calculations & statistics: Standard formulas for three- and four-point flexure, corrections (chamfer, thermal), and reporting of mean strength, standard deviation, and Weibull scaling (informative annex).
Applications and users
ISO 17565 is intended for:
- Materials scientists and ceramic engineers performing high-temperature mechanical characterization.
- Test laboratories and quality control teams in advanced ceramics manufacturing.
- R&D departments generating design allowable values or validating high-temperature performance of ceramic components (e.g., engine, turbine, sensor, or refractory applications).
- Standards bodies and accreditation labs needing reproducible, comparable elevated-temperature strength data.
Related standards
- ISO 14704:2000 - flexural strength of monolithic ceramics at room temperature.
- IEC 60584-1 - thermocouples: reference tables.
- ISO 7500-1 - verification/calibration of static uniaxial testing machines.
Keywords: ISO 17565, flexural strength, fine ceramics, elevated temperature testing, four-point flexure, thermocouple, high-temperature mechanical testing, ceramic composites.
Frequently Asked Questions
ISO 17565:2003 is a standard published by the International Organization for Standardization (ISO). Its full title is "Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for flexural strength of monolithic ceramics at elevated temperature". This standard covers: ISO 17565:2003 describes the method of test for determining the flexural strength of monolithic fine ceramics and whisker- or particulate-reinforced ceramic composites at elevated temperature. Flexural strength is one measure of the uniaxial strength of fine ceramics. This test method may be used for materials development, quality control, characterization and design data generation purposes.
ISO 17565:2003 describes the method of test for determining the flexural strength of monolithic fine ceramics and whisker- or particulate-reinforced ceramic composites at elevated temperature. Flexural strength is one measure of the uniaxial strength of fine ceramics. This test method may be used for materials development, quality control, characterization and design data generation purposes.
ISO 17565:2003 is classified under the following ICS (International Classification for Standards) categories: 81.060.30 - Advanced ceramics. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO 17565:2003 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
INTERNATIONAL ISO
STANDARD 17565
First edition
2003-12-15
Fine ceramics (advanced ceramics,
advanced technical ceramics) — Test
method for flexural strength of monolithic
ceramics at elevated temperature
Céramiques techniques — Méthode d'essai de résistance à la flexion
des céramiques monolithiques à température élevée
Reference number
©
ISO 2003
PDF disclaimer
This PDF file may contain embedded typefaces. In accordance with Adobe's licensing policy, this file may be printed or viewed but shall
not be edited unless the typefaces which are embedded are licensed to and installed on the computer performing the editing. In
downloading this file, parties accept therein the responsibility of not infringing Adobe's licensing policy. The ISO Central Secretariat
accepts no liability in this area.
Adobe is a trademark of Adobe Systems Incorporated.
Details of the software products used to create this PDF file can be found in the General Info relative to the file; the PDF-creation
parameters were optimized for printing. Every care has been taken to ensure that the file is suitable for use by ISO member bodies. In the
unlikely event that a problem relating to it is found, please inform the Central Secretariat at the address given below.
All rights reserved. Unless otherwise specified, no part of this publication may be reproduced or utilized in any form or by any means,
electronic or mechanical, including photocopying and microfilm, without permission in writing from either ISO at the address below or
ISO's member body in the country of the requester.
ISO copyright office
Case postale 56 CH-1211 Geneva 20
Tel. + 41 22 749 01 11
Fax + 41 22 749 09 47
E-mail copyright@iso.org
Web www.iso.org
Published in Switzerland
©
ii ISO 2003 – All rights reserved
Contents Page
1 Scope . 1
2 Normative references . 1
3 Terms and definitions . 1
4 Principle . 3
5 Apparatus . 3
5.1 Testing machine . 3
5.2 Heating device . 3
5.3 Temperature measuring and indicating instruments . 4
5.4 Testing fixture . 5
5.5 Micrometer . 9
6 Test pieces . 9
6.1 Test piece size . 9
6.2 Test piece preparation . 10
7 Procedure . 10
8 Calculation . 13
8.1 Standard formula for the flexural strength in four-point flexure . 13
8.2 Standard formula for the flexural strength in three-point flexure . 14
8.3 Corrections for chamfer size . 14
8.4 Corrections for thermal expansion . 14
8.5 Mean strength and standard deviation . 15
9 Accuracy and precision . 15
10 Test report . 15
11 Strength scaling factors . 16
Annex A (informative) General information . 17
Annex B (normative) Chamfer correction factors . 18
Annex C (normative) Corrections for thermal expansion . 21
Annex D (informative) Weibull scaling factors . 23
Annex E (informative) VAMAS round robin . 25
Bibliography . 26
©
ISO 2003 – All rights reserved iii
Foreword
ISO (the International Organization for Standardization) is a worldwide federation of national standards bodies
(ISO member bodies). The work of preparing International Standards is normally carried out through ISO
technical committees. Each member body interested in a subject for which a technical committee has been
established has the right to be represented on that committee. International organizations, governmental and
non-governmental, in liaison with ISO, also take part in the work. ISO collaborates closely with the International
Electrotechnical Commission (IEC) on all matters of electrotechnical standardization.
International Standards are drafted in accordance with the rules given in the ISO/IEC Directives, Part 2.
The main task of technical committees is to prepare International Standards. Draft International Standards
adopted by the technical committees are circulated to the member bodies for voting. Publication as an
International Standard requires approval by at least 75 % of the member bodies casting a vote.
Attention is drawn to the possibility that some of the elements of this document may be the subject of patent
rights. ISO shall not be held responsible for identifying any or all such patent rights.
ISO 17565 was prepared by Technical Committee ISO/TC 206, Fine ceramics.
©
iv ISO 2003 – All rights reserved
INTERNATIONAL STANDARD ISO 17565:2003(E)
Fine ceramics (advanced ceramics, advanced technical
ceramics) — Test method for flexural strength of monolithic
ceramics at elevated temperature
1Scope
This International Standard describes the method of test for determining the flexural strength of monolithic fine
ceramics and whisker- or particulate-reinforced ceramic composites at elevated temperature. Flexural strength
is one measure of the uniaxial strength of fine ceramics. This test method may be used for materials
development, quality control, characterization and design data generation purposes.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated
references, only the edition cited applies. For undated references, the latest edition of the referenced document
(including any amendments) applies.
ISO 3611:1978, Micrometer callipers for external measurement
1)
ISO 7500-1:— , Metallic materials — Verification of static uniaxial testing machines — Part1:
Tension/compression testing machines — Verification and calibration of the force-measuring system
ISO 14704:2000, Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for flexural
strength of monolithic ceramics at room temperature
IEC 60584-1:1995, Thermocouples — Part 1: Reference tables
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply.
3.1
flexural strength
maximum nominal stress at fracture of a specified elastic beam loaded in bending
3.2
four-point flexure
configuration of flexural strength testing where a test piece is equally loaded by two bearings symmetrically
located between two support bearings
See Figure 1.
NOTE The bearings may be cylindrical rollers or cylindrical bearings.
1) To be published. (Revision of ISO 7500-1:1999)
©
ISO 2003 – All rights reserved 1
a) Four-point-1/4 point flexure
b) Four-point-1/3 point flexure
c) Three-point flexure
Key
1 loading bearings
2 support bearing
Figure 1 — Flexural test configurations
3.3
four-point-1/4 point flexure
specific configuration of four-point flexural strength testing where the inner bearings are situated one quarter of
the support span away from the two outer bearings
See Figure 1 a).
©
2 ISO 2003 – All rights reserved
3.4
four-point-1/3 point flexure
specific configuration of four-point flexural strength testing where the inner bearings are situated one third of the
support span away from the two outer bearings
See Figure 1 b).
3.5
three-point flexure
configuration of flexural strength testing where a test piece is loaded at a location midway between two outer
bearings
See Figure 1 c).
NOTE Four-point flexure is usually preferred since a larger amount of material is exposed to the maximum stress. See
Bibliography for more information.
4 Principle
A beam test piece with a rectangular cross section is loaded in flexure until fracture. The load at fracture, the
test fixture and test piece dimensions are used to compute the flexural strength, which is a measure of the
uniaxial tensile strength of a ceramic. The material is assumed to be isotropic and linearly-elastic. Testing is
performed at elevated temperature in air or inert atmosphere. Load is monitored versus displacement or time in
order to confirm that the beam test piece fractured under elastic conditions. This International Standard is an
elevated-temperature adaptation of ISO 14704. See Annex A for additional information on this test method.
5 Apparatus
5.1 Testing machine
A suitable testing machine capable of applying a uniform crosshead speed shall be used. The testing machine
shall be in accordance with ISO 7500-1:— Class 1 with an accuracy of 1% of indicated load at fracture.
5.2 Heating device
5.2.1 General
The furnace shall be capable of heating the test fixture and test piece as well as maintaining a uniform and
constant temperature during the strength test. The furnace may have an air, inert gas or vacuum environment,
as required. If an inert gas or vacuum chamber is used, and it is necessary to transmit the load through a seal,
bellows or a fitting, it shall be verified that load losses or errors are less than 1% of the expected fracture loads.
The furnace may be designed so that test pieces are loaded into either hot or cold furnaces.
5.2.2 Test piece temperature stability
◦
The furnace shall be controlled by a device for maintaining a constant temperature within ± 2 C or better
within the working space of the furnace, during the time that the test piece is loaded to fracture.
5.2.3 Test piece temperature uniformity
The furnace shall be capable of maintaining the test piece temperature uniform. It shall previously be
◦
determined that the temperature of the test piece shall not vary more than 10 C over its length after a 15 min
hold time at the required test temperature.
©
ISO 2003 – All rights reserved 3
5.2.4 Furnace heating rate
The furnace control device shall also be capable of controlling the heating rates of the furnace and preventing
temperature overshoots.
5.2.5 Furnace stability
The time for the system to reach thermal equilibrium at test temperature shall be determined for the test
temperature to be used.
5.3 Temperature measuring and indicating instruments
5.3.1 General
◦
Thermocouple temperature measuring equipment shall have a resolution of at least 1 C and an accuracy of
◦ ◦ ◦
5 C or better. Optical pyrometers, if used, shall have a resolution of at least 5C5 and an accuracy of C or
better.
◦
NOTE 1 Resolution should not be confused with accuracy. Beware of instruments that have a resolution (read out) of 1 C,
◦ ◦ ◦
but have an accuracy of only 10C1; e.g., an instrument with a % accuracy would only be accurate to ± 12 C at 1 200 C.
NOTE 2 Thermocouple temperature measuring instruments typically approximate the temperature-electromotive force
(EMF) tables, but with a few degrees error.
5.3.2 Thermocouples
Thermocouples in accordance with IEC 60584-1 shall be used. The thermocouples shall exhibit low thermal
inertia (the diameter of the wires shall not be greater than 0,5 mm). The thermocouples shall have a sufficient
length within the furnace (with respect to heat conduction along the wires). The measuring thermocouple tip
shall be as close as possible to or contacting the test piece.
NOTE 1 In some furnaces, a control thermocouple may be installed at a location within the furnace which is convenient for
furnace control and a second measuring thermocouple may be in close proximity to the test piece.
NOTE 2 The thermocouple should not contact the test piece if there is a chance the test piece will be misaligned.
NOTE 3 The thermocouple should not contact the test piece if it will chemically react with the test piece.
5.3.3 Verification of the thermocouple temperature measuring system
Thermocouples shall be checked periodically since calibration may drift with usage or contamination.
5.3.4 Radiation pyrometers
Radiation pyrometers (thermometers) may be used in instances wherein suitable thermocouples are not
◦
available, particularly at temperatures above 1 600 C. Pyrometers may either be of the disappearing filament
type or an automatic type. Pyrometers may either be spectral (operate over a narrow wavelength band), dual
wavelength (operate over two narrow wavelength bands) or total (integrate or average over all wavelengths).
Radiation pyrometry requires special care in order to obtain accurate and precise results. Ensure that blackbody
conditions are obtained, or correct the temperature for the actual emissivity of the test piece in its environment.
The pyrometer should view the test piece at right angles to one of the four long surfaces. The target size (or
viewed area) of the pyrometer shall be less than 3mm in diameter. Corrections for radiation absorption or
reflectance may be necessary if the furnace has a window. The window shall be sufficiently large such that the
radiation emanating from the window completely fills the objective lens of the radiation thermometer, but the
window should not be so large as to cause appreciable heat loss or thermal gradients in the furnace.
NOTE See ASTM Standard Test Methods E 452, E 639, E 1256, and BS 1041, part 5 for additional information.
©
4 ISO 2003 – All rights reserved
5.4 Testing fixture
5.4.1 General
Three- or four-point flexure configurations shall be used as illustrated in Figures 1 and 2. The four-point-1/4-
point configuration is recommended. The fixtures shall either be semi-articulating or fully-articulating as
specified in ISO 14704 depending upon the condition of the test pieces. If the test pieces meet the parallelism
requirements of 6.1.1 and Figure 3, either a semi-articulating fixture or fully articulating fixture may be used. If
the test pieces do not meet the parallelism requirements of 6.1.1 and Figure 3, a fully-articulating fixture shall be
used.
NOTE 1 Machined test pieces normally have flat and parallel surfaces and semi-articulating fixtures are completely
satisfactory. On the other hand, as-fired, heated treated or oxidized test pieces often do not meet the parallelism
requirements. Twisting of the test piece can cause severe errors in the strength calculation, unless a fully-articulating fixture
is used. The purpose of articulation is to ensure that the bearings have uniform and even contact with the test piece surface.
NOTE 2 A fully-articulating fixture has bearings or rollers that are free to roll to eliminate friction. The bearings articulate
independently to match the test piece surface.
NOTE 3 A semi-articulating fixture has bearings or rollers that are free to roll to eliminate friction. The bearings articulate in
pairs to match the test piece surface.
It is recognized that practical limitations may restrict the design of the test fixture, and oxidation effects may
restrict its function. In such cases, alternatives may be employed, but deviations from the function specified
above shall be reported in the report.
5.4.2 Bearings
Test pieces shall be loaded and supported by bearings. The bearings shall be cylindrical rollers. The bearing
length shall be greater than or equal to 12 mm. The bearing diameter shall be approximately 1,5 times the test
piece thickness, h. Diameters between 4,5 mm and 5,0 mm are recommended. The bearings shall have a
smooth surface and shall have a diameter uniform to ± 0,015 mm. All bearings shall be free to roll in order to
eliminate friction, with the exception of the middle bearing in three point flexure (see Figure 2). For four-point
flexure, the two inner bearings shall be free to roll inwards, and the two outer bearings shall be free to roll
outwards. In three-point flexure, the two outer bearings shall be free to roll outwards, and the inner (middle)
bearing should not roll.
NOTE 1 Friction can cause errors in the stress calculations. The rolling action in elevated temperature fixtures is usually
accomplished by using cylindrical bearings which rest on a flat surface. The bearings are free to roll on the surface as shown
in Figure 2.
NOTE 2 The bearing diameter is specified on the basis of competing requirements. The bearings should not be so large as
to cause excessive change in the moment arm (“”a in Figure 1) as a test piece deflects which can create errors from contact-
point tangency shift. On the other hand, the bearings should not be so small as to create excessive wedging or contact
stresses in the test piece.
5.4.3 Four-point fixture — Semi-articulating
All four bearings shall be free to roll. The two inner bearings shall be parallel to each other to within 0,015 mm
over their length (� 12 mm in accordance with 5.4.2). The two outer bearings shall be parallel to each other to
within 0,015 mm over their length. The inner bearings shall be supported independently of the outer bearings.
All four bearings shall rest uniformly and evenly across the test piece surface. The fixture shall be designed to
apply equal loads to all four bearings.
NOTE The parallelism requirement may be met by control of the test fixture dimensions.
©
ISO 2003 – All rights reserved 5
The four bearings shall be free to roll in four-point flexure
a) Four-point flexure
The two outer bearings are free to roll outwards in the three-point flexure, but the middle bearing shall be non-
rolling
b) Three-point flexure
Key
1 test piece
2 alternative rolling bearings
3 alternatives
Figure 2 — Schematic of semi-articulating fixtures
©
6 ISO 2003 – All rights reserved
Dimensions in millimetres
a) The standard test piece
b) As-fired or heat treated test piece (see 6.1.2) — Specimen twist
c) As-fired or heat treated test piece (see 6.1.2) — Specimen bow
Key
1 one end on flat surface
2 gap
3bow
a
edge chamfers or rounding
Figure 3 — Test pieces
©
ISO 2003 – All rights reserved 7
5.4.4 Four-point fixture — Fully-articulating
All four bearings shall be free to roll. Three bearings shall articulate independently to match the test piece's
surface. The fourth bearing need not articulate. All four bearings shall rest uniformly and evenly across the test
piece surfaces. The fixture shall apply equal load to all four bearings.
5.4.5 Three-point fixture — Semi-articulating
The two support (outer) bearings shall be free to roll outwards. The middle bearing should be centrally located
and does not need to roll. The two outer bearings shall be parallel to each other to within 0,015 mm over their
length (� 12 mm in accordance with 5.4.2). The two outer bearings shall articulate together to match the test
piece surface or the middle bearing shall articulate to match the test piece surface. All three bearings shall rest
uniformly and evenly across the test piece surface. The fixture shall be designed to apply equal load to the two
outer bearings.
NOTE The parallelism requirement may be met by control of the test fixture dimensions.
5.4.6 Three-point fixture — Fully-articulating
The two support (outer) bearings shall be free to roll outwards. The middle bearing should not roll. Any two of
the bearings shall be capable of articulating independently to match the test piece surface. All three bearings
shall rest uniformly and evenly across the test piece surface. The fixture shall be designed to apply equal loads
to the two outer bearings.
5.4.7 Positioning of bearings
The bearings shall be positioned so that the spans have the prescribed dimensions to within ± 0,10 mm. The
middle bearing for the three-point fixture shall be positioned midway between the outer bearings to within
± 1,00 mm. The inner bearings for the four-point fixture shall be centred between the outer bearings to within
± 0,10 mm.
NOTE 1 The positions of the bearings may be defined either by the use of captive bearings, or by appropriate stops against
which the bearings are held at the commencement of a test. The spans may be measured to the nearest 0,1 mm using a
travelling microscope or other suitable device. The spans may also be verified by measurement of the distances between
bearing stops and adding (outer span) or subtracting (inner span) the radii of the bearing cylinders.
NOTE 2 Some fixtures have bearings that fit into square slots with a slight clearance. Of course, the clearance should be
such that the possible spans are within the prescribed limits of this International Standard. Unfortunately, it is usually not
possible to verify whether a bearing sits against an inner or outer shoulder, and thus it is possible that some bearings are
free to roll and others are not. This can lead to the addition of unpredictable, random friction errors. Fixtures with such slots
should be used with caution.
5.4.8 Fixture material
The fixture material shall be as inert as possible for the testing conditions used. The fixture shall be oxidation
resistant if the testing is done in air. The fixture shall have negligible chemical reaction with and shall not
contaminate the test piece. The fixture shall remain elastic over the load and temperature ranges used. The
bearings may be made of a ceramic with an elastic modulus between 200 GPa and 500 GPa and a flexural
strength greater than 275 GPa at elevated temperature.
NOTE 1 Bearings should be cleaned regularly. Silicon carbide papers are helpful in cleaning scale, oxidation products or
chemical reaction products off the fixtures.
NOTE 2 Various grades of silicon carbide or sapphire are suitable. Hot-pressed or sintered silicon carbides with low
◦
additive content are elastic up to temperatures in excess of 1 500 C. Siliconized silicon carbides and high purity aluminas
◦
are less expensive, but may exhibit creep deformation at temperatures over 1 200 C. Recrystallized silicon carbides are
◦
elastic up to temperatures of 2 000 C, but are relatively weak due to porosity. Graphites are extremely refractory but are
restricted to inert atmospheres and are soft and have a low elastic modulus. Graphites may be suitable for loading rams or
portions of fixtures, but they should not be used where there are concentrated loads such as at the loading bearings.
©
8 ISO 2003 – All rights reserved
NOTE 3 In some instances it may be suitable to use bearings made of a different material than the test fixture; e.g.,
sintered silicon carbide bearings may be used with hot-pressed silicon carbide fixtures. The sintered silicon carbide is brittle
and may have intermediate strength, but has low additive content and is highly oxidation resistant. The hot-pressed silicon
carbide is much stronger but may oxidize and react with the test piece.
5.4.9 Fixture compliance
It is recommended that the compliance of the load train be characterized for the loading range and temperature
used. An oversized ceramic block may be inserted into the fixture and loaded to the maximum expected
breaking load at the test temperature. The load train and fixture shall be sufficiently rigid that at least 70 % of the
crosshead motion is transmitted to the ceramic test pieces.
5.5 Micrometer
A micrometer such as is shown in ISO 3611 but with a resolution of 0,002 mm shall be used to measure the test
piece dimensions. The micrometer shall have flat anvils. The micrometer shall not have a ball tip or sharp tip
since these might damage the test piece. Alternative dimension measuring instruments may be used provided
0,002 mm
that they have a resolution of or finer.
6 Test pieces
6.1 Test piece size
6.1.1 Machined test pieces
Test pieces shall be prepared in accordance with ISO 14704. Test piece dimensions are shown in Figure 3.
Cross-sectional tolerances shall be ± 0,5 mm. The parallelism tolerance on opposite longitudinal faces is
0,015 mm.
6.1.2 As-fired or heat-treated test pieces
Test piece dimensions may be altered as required. Test piece dimensions are shown in Figure 3, except that
cross section sizes shall be within ± 0,5 mm of the prescribed dimensions. The initial curvature of a test piece
for 4-point loading shall be such that any specimen bow shall be less than 0,4 mm as shown in Figure 3 c). The
bow shall be less than for 3-point testing on outer spans, or less than for 3-point testing
0,8 mm 30 mm 1,3 mm
on 40 mm outer spans. In addition, the 4 mm wide surfaces which contact the bearings shall have a flatness of
0,15 mm
or smaller. Deviations from the specifications in 6.1.1 and Figure 3 shall be stated in the report.
Special note shall be made if the test pieces are twisted in which case an estimate of the twist angle along the
length of the test piece shall be reported.
NOTE 1 Very twisted [Figure 3 b)] or bowed [Figure 3 c)] test pieces may interfere with proper test fixture articulation with
an attendant loss of accuracy and precision. The intrinsic error associated with testing test pieces with an initial curvature is
quite small and is usually much less than 1% [6]. Surface reaction layers or irregularities may also interfere with proper force
distribution in the test fixtures.
NOTE 2 Test piece twist may be estimated by holding one end of the test piece on a flat surface and observing the opposite
end of the test piece. If the test piece is twisted, one edge will be raised up off the flat surface. The gap between the raised
test piece end and the flat surface may be estimated by inserting thickness shims of various sizes. The test piece twist is
−1
sin (gap/4). See Figure 3 b).
NOTE 3 Some fully-articulating fixtures may have limitations in the ability to accommodate twisted test pieces. Users
should be aware of these limitations if they exist, and avoid testing pieces with excessive twists.
©
ISO 2003 – All rights reserved 9
6.2 Test piece preparation
6.2.1 General
This International Standard allows several options for test piece preparation. In all cases, the end faces of the
test piece do not need special preparation or finishing. A minimum of two long edges, on one 4mm wide face,
shall be chamfered or rounded as shown in Figure 3. It is highly recommended that all four long edges be
chamfered or rounded. Although a surface finish specification is not part of this International Standard, it is
highly recommended that the surface roughness be measured and reported. Test pieces may be:
a) as-fired;
b) machined by a customary-machining procedure;
c) machined by a component-matched procedure;
d) machined by the basic procedure defined in ISO 14704:2000, clause 6.2.5.
Consult ISO 14704 for additional details for these four options.
NOTE Surface preparation of test pieces can introduce machining flaws (especially microcracks beneath the test piece
surface) which may have a pronounced effect on flexural strength. Machining damage can either be a random interfering
factor, or an inherent part of the strength characteristics to be measured. Surface preparation can also create residual
stresses. Final machining steps (including polishing) may or may not negate machining damage introduced from prior,
coarser machining steps.
6.2.2 Chamfers
◦
The long edges shall be uniformly chamfered at 45 to a size of 0,12 mm± 0,03 mm as shown in Figure 3.
They can alternatively be rounded with a radius of 0,15 mm± 0,05 mm. Edge chamfering or rounding shall be
comparable to that applied to the test piece surfaces in the fine finishing step. The direction of machining shall
be parallel to the test piece long axis. The maximum chamfer size permitted in this International Standard will
cause a 1% error in flexure strength. If for some reason the chamfers are larger than the specified size range
(e.g., for the removal of very large chips), then the stresses shall be corrected for the reduced second moment
of inertia of the test piece cross section in accordance with Annex B. As-fired test pieces may have chamfers
applied before firing.
6.2.3 Test piece storage
The test pieces shall be handled with care to avoid the introduction of damage after test piece preparation. Test
pieces shall be stored separately and not allowed to impact or scratch each other.
6.2.4 Number of test pieces
A minimum of 10 test pieces shall be required for the purpose of estimating the mean flexural strength. A
minimum of 30 test pieces shall be used if a statistical strength analysis (e.g., a Weibull analysis) is made.
NOTE The use of 30 test pieces will help obtain good confidence limits for the strength distribution parameters such as a
Weibull modulus. 30 test pieces will also hel
...