Aluminium and aluminium alloys - Chemical composition and form of wrought products - Part 3: Chemical composition and form of products

This European Standard specifies the chemical composition limits of wrought aluminium and wrought aluminium alloys and form of products.
The chemical composition limits of aluminium and aluminium alloys specified herein are completely identical with those registered with the Aluminum Association, 1525, Wilson Boulevard, Suite 600, Arlington, VA 22209, USA, for the corresponding alloys.

Aluminium und Aluminiumlegierungen - Chemische Zusammensetzung und Form von Halbzeug - Teil 3: Chemische Zusammensetzung und Erzeugnisformen

Diese Europäische Norm legt die Grenzwerte für die chemische Zusammensetzung von Aluminium und Aluminium-Knetlegierungen und die Erzeugnisformen fest.
Die hier festgelegten Grenzwerte für die chemische Zusammensetzung von Aluminium und Aluminiumlegierungen stimmen völlig mit den entsprechenden Legierungen überein, die bei der Aluminum Association, 1525, Wilson Boulevard, Suite 600, Arlington, VA 22209, USA, registriert sind.

Aluminium et alliages d'aluminium - Composition chimique et forme des produits corroyés - Partie 3 : Composition chimique et forme des produits

Cette Norme européenne spécifie les limites de composition chimique des aluminiums et alliages d’aluminium corroyés et les formes de produits.
Les limites de composition chimique de l’aluminium et des alliages d’aluminium spécifiées ici sont strictement identiques à celles enregistrées auprès de l’Aluminium Association, 1525 Wilson Boulevard, Suite 600, Arlington, VA 22209, États-Unis, pour les alliages correspondants.

Aluminij in aluminijeve zlitine - Kemična sestava in oblika gnetenih izdelkov - 3. del: Kemična sestava in oblika izdelkov

General Information

Status
Withdrawn
Publication Date
09-Jun-2009
Withdrawal Date
07-Jan-2014
Technical Committee
Current Stage
9900 - Withdrawal (Adopted Project)
Start Date
07-Jan-2014
Due Date
30-Jan-2014
Completion Date
08-Jan-2014

Relations

Buy Standard

Standard
EN 573-3:2009
English language
36 pages
sale 10% off
Preview
sale 10% off
Preview
e-Library read for
1 day

Standards Content (Sample)

SLOVENSKI STANDARD
SIST EN 573-3:2009
01-julij-2009
1DGRPHãþD
SIST EN 573-3:2007
$OXPLQLMLQDOXPLQLMHYH]OLWLQH.HPLþQDVHVWDYDLQREOLNDJQHWHQLKL]GHONRY
GHO.HPLþQDVHVWDYDLQREOLNDL]GHONRY
Aluminium and aluminium alloys - Chemical composition and form of wrought products -
Part 3: Chemical composition and form of products
Aluminium und Aluminiumlegierungen - Chemische Zusammensetzung und Form von
Halbzeug - Teil 3: Chemische Zusammensetzung und Erzeugnisformen
Aluminium et alliages d'aluminium - Composition chimique et forme des produits
corroyés - Partie 3 : Composition chimique et forme des produits
Ta slovenski standard je istoveten z: EN 573-3:2009
ICS:
77.040.30 Kemijska analiza kovin Chemical analysis of metals
77.150.10 Aluminijski izdelki Aluminium products
SIST EN 573-3:2009 en,fr,de
2003-01.Slovenski inštitut za standardizacijo. Razmnoževanje celote ali delov tega standarda ni dovoljeno.

---------------------- Page: 1 ----------------------

SIST EN 573-3:2009

---------------------- Page: 2 ----------------------

SIST EN 573-3:2009
EUROPEAN STANDARD
EN 573-3
NORME EUROPÉENNE
EUROPÄISCHE NORM
April 2009
ICS 77.120.10; 77.150.10 Supersedes EN 573-3:2007
English Version
Aluminium and aluminium alloys - Chemical composition and
form of wrought products - Part 3: Chemical composition and
form of products
Aluminium et alliages d'aluminium - Composition chimique Aluminium und Aluminiumlegierungen - Chemische
et forme des produits corroyés - Partie 3 : Composition Zusammensetzung und Form von Halbzeug - Teil 3:
chimique et forme des produits Chemische Zusammensetzung und Erzeugnisformen
This European Standard was approved by CEN on 19 March 2009.
CEN members are bound to comply with the CEN/CENELEC Internal Regulations which stipulate the conditions for giving this European
Standard the status of a national standard without any alteration. Up-to-date lists and bibliographical references concerning such national
standards may be obtained on application to the CEN Management Centre or to any CEN member.
This European Standard exists in three official versions (English, French, German). A version in any other language made by translation
under the responsibility of a CEN member into its own language and notified to the CEN Management Centre has the same status as the
official versions.
CEN members are the national standards bodies of Austria, Belgium, Bulgaria, Cyprus, Czech Republic, Denmark, Estonia, Finland,
France, Germany, Greece, Hungary, Iceland, Ireland, Italy, Latvia, Lithuania, Luxembourg, Malta, Netherlands, Norway, Poland, Portugal,
Romania, Slovakia, Slovenia, Spain, Sweden, Switzerland and United Kingdom.
EUROPEAN COMMITTEE FOR STANDARDIZATION
COMITÉ EUROPÉEN DE NORMALISATION
EUROPÄISCHES KOMITEE FÜR NORMUNG
Management Centre: Avenue Marnix 17, B-1000 Brussels
© 2009 CEN All rights of exploitation in any form and by any means reserved Ref. No. EN 573-3:2009: E
worldwide for CEN national Members.

---------------------- Page: 3 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Contents Page
Foreword .3
1 Scope .4
2 Normative references .4
3 Chemical composition limits .4
4 Writing rules .4
5 Alloy designations .5
6 Sequence of elements .5
7 Rounding rules for determination of compliance .5
Annex A (normative) Form of products . 20
A.1 General . 20
A.2 European Standards . 20
Annex B (normative) Guidelines for the introduction of new wrought aluminium and wrought
aluminium alloys in CEN/TC 132 standards . 34
B.1 General principles. 34
B.2 Rules for introduction of new alloys. 34
B.3 Procedure for introduction of new alloys . 34
B.4 Addendum for new alloys for future introduction . 34
Bibliography . 35

2

---------------------- Page: 4 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Foreword
This document (EN 573-3:2009) has been prepared by Technical Committee CEN/TC 132 “Aluminium and
aluminium alloys”, the secretariat of which is held by AFNOR.
This European Standard shall be given the status of a national standard, either by publication of an identical
text or by endorsement, at the latest by October 2009, and conflicting national standards shall be withdrawn at
the latest by October 2009.
Attention is drawn to the possibility that some of the elements of this document may be the subject of patent
rights. CEN [and/or CENELEC] shall not be held responsible for identifying any or all such patent rights.
CEN/TC 132 affirms its policy that if a patentee refuses to grant licenses on standardised products under
reasonable and not discriminatory conditions, this product will be removed from the corresponding document.
This document supersedes EN 573-3:2007.
Within its programme of work, Technical Committee CEN/TC 132 entrusted CEN/TC 132/WG 7 "Sheets,
strips and plates" to revise EN 573-3:2007.
CEN/TC 132 has decided to revise this standard every two years if necessary. The following modifications
have been introduced during the revision:
 Clause 3: the last sentence was re-written to be clear;
 Tables 1 to 8 and Tables A.1 to A.8: in the column "Chemical symbol", suffixes (A), (B) and (C) were
re-inserted;
 Table 5 and Table A.5 : in the column "Chemical symbol", the suffix (D) was re-inserted;
 Table 1 and Table A.1: alloy EN AW-1110 was added;
 Table 8 and Table A.8: alloys EN AW-8030 and EN AW-8176 were added.
 EN 573 comprises the following parts under the general title "Aluminium and aluminium alloys —
Chemical composition and form of wrought products":
 Part 1: Numerical designation system
 Part 2: Chemical symbol based designation system
 Part 3: Chemical composition and form of products
 Part 4: Forms of products
 Part 5: Codification of standardized wrought products
According to the CEN/CENELEC Internal Regulations, the national standards organizations of the following
countries are bound to implement this European Standard: Austria, Belgium, Bulgaria, Cyprus, Czech
Republic, Denmark, Estonia, Finland, France, Germany, Greece, Hungary, Iceland, Ireland, Italy, Latvia,
Lithuania, Luxembourg, Malta, Netherlands, Norway, Poland, Portugal, Romania, Slovakia, Slovenia, Spain,
Sweden, Switzerland and the United Kingdom.
3

---------------------- Page: 5 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
1 Scope
This European Standard specifies the chemical composition limits of wrought aluminium and wrought
aluminium alloys and form of products.
The chemical composition limits of aluminium and aluminium alloys specified herein are completely identical
with those registered with the Aluminum Association, 1525, Wilson Boulevard, Suite 600, Arlington, VA 22209,
USA, for the corresponding alloys.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated
references, only the edition cited applies. For undated references, the latest edition of the referenced
document (including any amendments) applies.
EN 573-2, Aluminium and aluminium alloys — Chemical composition and form of wrought products —
Part 2: Chemical symbol based designation system
3 Chemical composition limits
The chemical composition of aluminium and aluminium alloys is specified in percentage by mass in Tables 1
to 8. Limits of impurities are expressed as a maximum; limits of alloying elements shown as a range
aluminium is specified as a minimum for unalloyed aluminium, and as a remainder for aluminium alloys.
The chemical composition of internationally registered wrought aluminium and wrought aluminium alloys not
listed in this document can be found in Teal sheet [1].
Analysis shall be made for elements which are specified, for example Pb, Sn, Bi, Sb, Zr.
4 Writing rules
4.1 Standard limits for alloying elements and impurities are expressed in percentage by mass to the
following decimal places:
 less than 0,001 % 0,000X;
 0,001 % but less than 0,01 % 0,00X;
 0,01 % but less than 0,10 %:
 unalloyed aluminium made by a refining process 0,0XX;
 others 0,0X;
 0,10 % to 0,55 % 0,XX;
 over 0,55 % 0,X; X,X; XX,X.
Exception: combined Si + Fe limits for 1xxx designations shall be expressed as 0,XX or 1,XX.
4.2 The aluminium content for unalloyed aluminium made by a refining process is the difference
between 100,00 % and the sum of all other metallic elements present in amounts of 0,0010 % or more each,
4

---------------------- Page: 6 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
expressed to the third decimal place before determining the sum, which is rounded to the second decimal
place before subtracting.
For unalloyed aluminium not made by a refining process, the aluminium content is the difference
between 100,00 % and the sum of all other metallic elements present in amounts of 0,010 % or more each
expressed to the second decimal place before determining the sum.
5 Alloy designations
The numerical designation systems used in Teal sheets and European Standards for wrought aluminium
alloys are identical. As specified in EN 573-1 the prefix EN AW- is added.
The alternative chemical symbol based alloy designation system shall be based on EN 573-2.
Both the numerical and the chemical symbol based designations are indicated in Tables 1 to 8.
The International numerical system is the preferred one. The chemical symbol based designations are
indicated for reference only.
6 Sequence of elements
Standard limits for alloying elements and impurities are expressed in the following sequence: silicon, iron,
copper, manganese, magnesium, chromium, nickel, zinc, titanium, gallium, vanadium, remarks, other
elements each, other elements total, aluminium.
Limits of additional specified elements are inserted in alphabetical order of their chemical symbols under
“Remarks”.
7 Rounding rules for determination of compliance
In recording chemical analysis test results, the number representing the result for any element specified in this
standard shall be expressed to the same number of decimal places as the corresponding number in this
standard. For unalloyed aluminium, the aluminium content is derived as described in 4.2.
The following rounding rules shall be used for determination of compliance with this standard:
a) when the figure immediately after the last figure to be retained is less than 5, the last figure to be retained
remains unchanged;
b) when the figure immediately after the last figure to be retained is greater than 5, or equal to 5 and
followed by at least one figure other than zero, the last figure to be retained is increased by one;
c) when the figure immediately after the last figure to be retained is equal to 5 and followed by zeros only,
the last figure to be retained remains unchanged if even and is increased by one if odd.
5

---------------------- Page: 7 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 1 — Aluminium — 1 000 series
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
Chemical
b
Numerical Each Total min.
symbols
c
EN AW-1050A EN AW-Al 99,5 0,25 0,40 0,05 0,05 0,05 - - 0,07 0,05 - - - 0,03 -
99,50
c
EN AW-1060 EN AW-Al 99,6 0,25 0,35 0,05 0,03 0,03 - - 0,05 0,03 - 0,05 - 0,03 -
99,60
c
EN AW-1070A EN AW-Al 99,7 0,20 0,25 0,03 0,03 0,03 - - 0,07 0,03 - - - 0,03 -
99,70
c
e
EN AW-1080A EN AW-Al 99,8(A) 0,15 0,15 0,03 0,02 0,02 - - 0,06 0,02 0,03 - 0,02 -
99,80

c
EN AW-1085 EN AW-Al 99,85 0,10 0,12 0,03 0,02 0,02 - - 0,03 0,02 0,03 0,05 - 0,01 -
99,85
c
EN AW-1090 EN AW-Al 99,90 0,07 0,07 0,02 0,01 0,01 - - 0,03 0,01 0,03 0,05 - 0,01 -
99,90
d
EN AW-1098 EN AW-Al 99,98 0,010 0,006 0,003 - - - - 0,015 0,003 - - - 0,003 -
99,98
c
EN AW-1100 EN AW-Al 99,0Cu 0,95 Si + Fe 0,05-0,20 0,05 - - - 0,10 - - - e 0,05 0,15
99,00

c

EN AW-1110
EN AW-Al 99,1 0,30 0,8 0,04 0,01 0,25 0,01 – – – – – 0,02B; 0,03V + Ti 0,03 0,15
99,10
d
EN AW-1198 EN AW-Al 99,98(A) 0,010 0,006 0,006 0,006 - - - 0,010 0,006 0,006 - - 0,003 -
99,98
d
EN AW-1199 EN AW-Al 99,99 0,006 0,006 0,006 0,002 0,006 - - 0,006 0,002 0,005 0,005 - 0,002 -
99,99
c
e
EN AW-1200 EN AW-Al 99,0 1,00 Si + Fe 0,05 0,05 - - - 0,10 0,05 - - 0,05 0,15 99,00

c
EN AW-1200A EN AW-Al 99,0(A) 1,00 Si + Fe 0,10 0,30 0,30 0,10 - 0,10 - - - - 0,05 0,15 99,00
c
EN AW-1235 EN AW-Al 99,35 0,65 Si + Fe 0,05 0,05 0,05 - - 0,10 0,06 - 0,05 - 0,03 - 99,35
c
EN AW-1350 EN AW-Al 99,5 0,10 0,40 0,05 0,01 - 0,01 - 0,05 - 0,03 - 0,05 B; 0,02 V + Ti 0,03 0,10
99,50
c
EN AW-1350A EN AW-Al 99,5(A) 0,25 0,40 0,02 - 0,05 - - 0,05 - - - 0,03 Cr + Mn + Ti + V 0,03 -
99,50

6

---------------------- Page: 8 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 1 — Aluminium — 1 000 series (continued)
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
Chemical
b
Numerical Each Total min.
symbols
c
EN AW-1370 EN AW-Al 99,7 0,10 0,25 0,02 0,01 0,02 0,01 - 0,04 - 0,03 - 0,02 B; 0,02 V + Ti 0,02 0,10
99,70
c
e
EN AW-1450 EN AW-Al 99,5Ti 0,25 0,40 0,05 0,05 0,05 - - 0,07 0,10-0,20 - - 0,03 -
99,50



a
 "Others" includes listed elements for which no specific limit is shown as well as unlisted metallic elements. The producer may analyze samples for trace elements not specified in the registration or specification. However, such
analysis is not required and may not cover all metallic "Other" elements. Should any analysis by the producer or the purchaser establish that an "Others" element exceeds the limit of "Each" or that the aggregate of several "Others"
elements exceeds the limit of "Total", the material shall be considered non-conforming.
b
The sum of those "Others" metallic elements 0,010 % or more each, expressed to the second decimal place before determining the sum.
c
The aluminium content for unalloyed aluminium not made by a refining process is the difference between 100,00 % and the sum of all other metallic elements present in amounts of 0,010 % or more each, expressed to the second
decimal place before determining the sum.
d
The aluminium content for unalloyed aluminium made by a refining process is the difference between 100,00 % and the sum of all other metallic elements present in amounts of 0,0010 % or more each, expressed to the third decimal
before determining the sum, which is rounded to the second decimal place before subtracting.
e
0,0003 max. Be for welding electrode, welding rod and filler wire only.


7

---------------------- Page: 9 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 2 — Aluminium alloys — 2 000 series — Al Cu
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
b
Numerical Chemical symbols Each min.
Total
c
EN AW-2001 EN AW-Al Cu5,5MgMn 0,20 0,20 5,2-6,0 0,15-0,50 0,20-0,45 0,10 0,05 0,10 0,20 - - 0,05 0,15 Remainder
0,05 Zr
d
EN AW-2007 EN AW-Al Cu4PbMgMn 0,8 0,8 3,3-4,6 0,50-1,0 0,40-1,8 0,10 0,20 0,8 0,20 - - 0,10 0,30 Remainder
e
EN AW-2011 EN AW-Al Cu6BiPb 0,40 0,7 5,0-6,0 - - - - 0,30 - - - 0,05 0,15 Remainder
e
EN AW-2011A EN AW-Al Cu6BiPb(A) 0,40 0,50 4,5-6,0 - - - - 0,30 - - - 0,05 0,15 Remainder
f
-
EN AW-2014 EN AW-Al Cu4SiMg 0,50-1,2 0,7 3,9-5,0 0,40-1,2 0,20-0,8 0,10 - 0,25 0,15 - 0,05 0,15 Remainder
EN AW-2014A EN AW-Al Cu4SiMg(A) 0,50-0,9 0,50 3,9-5,0 0,40-1,2 0,20-0,8 0,10 0,10 0,25 0,15 - - 0,20 Zr+Ti 0,05 0,15 Remainder
EN AW-2017A EN AW-Al Cu4MgSi(A) 0,20-0,8 0,7 3,5-4,5 0,40-1,0 0,40-1,0 0,10 - 0,25 - - - 0,25 Zr+Ti 0,05 0,15 Remainder
f
EN AW-2024 EN AW-Al Cu4Mg1 0,50 0,50 3,8-4,9 0,30-0,9 1,2-1,8 0,10 - 0,25 0,15 - - 0,05 0,15 Remainder
0,20 Bi ; 0,8-1,5
EN AW-2030 EN AW-Al Cu4PbMg 0,8 0,7 3,3-4,5 0,20-1,0 0,50-1,3 0,10 - 0,50 0,20 - - 0,10 0,30 Remainder
Pb
EN AW-2031 EN AW-Al Cu2,5NiMg 0,50-1,3 0,6-1,2 1,8-2,8 0,50 0,6-1,2 - 0,6-1,4 0,20 0,20 - - - 0,05 0,15 Remainder
g
EN AW-2091 EN AW-Al Cu2Li2Mg1,5 0,20 0,30 1,8-2,5 0,10 1,1-1,9 0,10 - 0,25 0,10 - - 0,04-0,16 Zr 0,05 0,15 Remainder
EN AW-2117 EN AW-Al Cu2,5Mg 0,8 0,7 2,2-3,0 0,20 0,20-0,50 0,10 - 0,25 - - - - 0,05 0,15 Remainder
f
EN AW-2124 EN AW-Al Cu4Mg1(A) 0,20 0,30 3,8-4,9 0,30-0,9 1,2-1,8 0,10 - 0,25 0,15 - - 0,05 0,15 Remainder
f
EN AW-2214 EN AW-Al Cu4SiMg(B) 0,50-1,2 0,30 3,9-5,0 0,40-1,2 0,20-0,8 0,10 - 0,25 0,15 - - 0,05 0,15 Remainder
EN AW-2219 EN AW-Al Cu6Mn 0,20 0,30 5,8-6,8 0,20-0,40 0,02 - - 0,10 0,02-0,10 - 0,05-0,15 0,10-0,25 Zr 0,05 0,15 Remainder

8

---------------------- Page: 10 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 2 — Aluminium alloys — 2 000 series — Al Cu (continued)
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
b
Numerical Chemical symbols Each min.
Total
h
EN AW-2319 EN AW-Al Cu6Mn(A) 0,20 0,30 5,8-6,8 0,20-0,40 0,02 - - 0,10 0,10-0,20 - 0,05-0,15 0,05 0,15 Remainder
0,10-0,25 Zr
EN AW-2618A EN AW-Al Cu2Mg1,5Ni 0,15-0,25 0,9-1,4 1,8-2,7 0,25 1,2-1,8 - 0,8-1,4 0,15 0,20 - - 0,25 Zr+Ti 0,05 0,15 Remainder

a
"Others" includes listed elements for which no specific limit is shown as well as unlisted metallic elements. The producer may analyze samples for trace elements not specified in the registration or specification. However, such
analysis is not required and may not cover all metallic "Other" elements. Should any analysis by the producer or the purchaser establish that an "Others" element exceeds the limit of "Each" or that the aggregate of several "Others"
elements exceeds the limit of "Total", the material shall be considered non-conforming.
b
The sum of those "Others" metallic elements 0,010 % or more each, expressed to the second decimal place before determining the sum.
c
0,003 max. Pb.
d
0,20 Bi; 0,8-1,5 Pb; 0,20 Sn.
e
0,20-0,6 Bi; 0,20-0,6 Pb.
f
Zr + Ti limit of 0,20 maximum may be used for extruded and forged products if mutually agreed by supplier or manufacturer and purchaser.
g
1,7-2,3 Li.
h
0,0003 max. Be for welding electrode, welding rod and filler wire only.

9

---------------------- Page: 11 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 3 — Aluminium alloys — 3 000 series — Al Mn
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
b
Numerical Chemical Symbols Each min.
Total
EN AW-3002 EN AW-Al Mn0,2Mg0,1 0,08 0,10 0,15 0,05-0,25 0,05-0,20 - - 0,05 0,03 - 0,05 - 0,03 0,10 Remainder
EN AW-3003 EN AW-Al Mn1Cu 0,6 0,7 0,05-0,20 1,0-1,5 - - - 0,10 - - - - 0,05 0,15 Remainder
EN AW-3004 EN AW-Al Mn1Mg1 0,30 0,7 0,25 1,0-1,5 0,8-1,3 - - 0,25 - - - - 0,05 0,15 Remainder
EN AW-3005 EN AW-Al Mn1Mg0,5 0,6 0,7 0,30 1,0-1,5 0,20-0,6 0,10 - 0,25 0,10 - - - 0,05 0,15 Remainder
EN AW-3005A EN AW-Al Mn1Mg0,5(A) 0,7 0,8 0,30 1,0-1,5 0,20-0,6 0,10 - 0,40 0,10 - - - 0,05 0,15 Remainder
EN AW-3017 EN AW-Al Mn1Cu0,3 0,25 0,25-0,45 0,25-0,40 0,8-1,2 0,10 0,15 - 0,10 0,05 - - - 0,05 0,15 Remainder
EN AW-3102 EN AW-Al Mn0,2 0,40 0,7 0,10 0,05-0,40 - - - 0,30 0,10 - - - 0,05 0,15 Remainder
c
EN AW-3103 EN AW-Al Mn1 0,50 0,7 0,10 0,9-1,5 0,30 0,10 - 0,20 - - - 0,05 0,15 Remainder
0,10 Zr+Ti
EN AW-3103A EN AW-Al Mn1(A) 0,50 0,7 0,10 0,7-1,4 0,30 0,10 - 0,20 0,10 - - 0,10 Zr+Ti 0,05 0,15 Remainder
EN AW-3104 EN AW-Al Mn1Mg1Cu 0,6 0,8 0,05-0,25 0,8-1,4 0,8-1,3 - - 0,25 0,10 0,05 0,05 - 0,05 0,15 Remainder
EN AW-3105 EN AW-Al Mn0,5Mg0,5 0,6 0,7 0,30 0,30-0,8 0,20-0,8 0,20 - 0,40 0,10 - - - 0,05 0,15 Remainder
EN AW-3105A EN AW-Al Mn0,5Mg0,5(A) 0,6 0,7 0,30 0,30-0,8 0,20-0,8 0,20 - 0,25 0,10 - - - 0,05 0,15 Remainder
EN AW-3105B EN AW-Al Mn0,6Mg0,5 0,7 0,9 0,30 0,30-0,9 0,20-0,8 0,20 - 0,50 0,10 - - 0,10 Pb 0,05 0,15 Remainder
EN AW-3207 EN AW-Al Mn0,6 0,30 0,45 0,10 0,40-0,8 0,10 - - 0,10 - - - - 0,05 0,10 Remainder
EN AW-3207A EN AW-Al Mn0,6(A) 0,35 0,6 0,25 0,30-0,8 0,40 0,20 - 0,25 - - - - 0,05 0,15 Remainder
a
 "Others" includes listed elements for which no specific limit is shown as well as unlisted metallic elements. The producer may analyze samples for trace elements not specified in the registration or specification. However, such
analysis is not required and may not cover all metallic "Other" elements. Should any analysis by the producer or the purchaser establish that an "Others" element exceeds the limit of "Each" or that the aggregate of several "Others"
elements exceeds the limit of "Total", the material shall be considered non-conforming.
b
The sum of those "Others" metallic elements 0,010 % or more each, expressed to the second decimal place before determining the sum.
c
0,0003 max. Be for welding electrode, welding rod and filler wire only.

10

---------------------- Page: 12 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 4 — Aluminium alloys — 4 000 series — Al Si
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
b
Numerical Chemical symbols Each min.
Total
EN AW-4004 EN AW-Al Si10Mg1,5 9,0-10,5 0,8 0,25 0,10 1,0-2,0 - - 0,20 - - - - 0,05 0,15 Remainder
EN AW-4006 EN AW-Al Si1Fe 0,8-1,2 0,50-0,8 0,10 0,05 0,01 0,20 - 0,05 - - - - 0,05 0,15 Remainder
EN AW-4007 EN AW-Al Si1,5Mn 1,0-1,7 0,40-1,0 0,20 0,8-1,5 0,20 0,05-0,25 0,15-0,7 0,10 0,10 - - 0,05 Co 0,05 0,15 Remainder
EN AW-4015 EN AW-Al Si2Mn 1,4-2,2 0,7 0,20 0,6-1,2 0,10-0,50 - - 0,20 - - - - 0,05 0,15 Remainder
EN AW-4016 EN AW-Al Si2MnZn 1,4-2,2 0,7 0,20 0,6-1,2 0,10 - - 0,50-1,3 - - - - 0,05 0,15 Remainder
EN AW-4017 EN AW-Al SiMnMgCu 0,6-1,6 0,7 0,10-0,50 0,6-1,2 0,10-0,50 - - 0,20 - - - - 0,05 0,15 Remainder
c
EN AW-4018 EN AW-Al Si7Mg 6,5-7,5 0,20 0,05 0,10 0,50-0,8 - - 0,10 0,20 - - 0,05 0,15 Remainder
EN AW-4032 EN AW-Al Si12,5MgCuNi 11,0-13,5 1,0 0,50-1,3 - 0,8-1,3 0,10 0,50-1,3 0,25 - - - - 0,05 0,15 Remainder
c
EN AW-4043A EN AW-Al Si5(A) 4,5-6,0 0,6 0,30 0,15 0,20 - - 0,10 0,15 - - 0,05 0,15 Remainder
EN AW-4045 EN AW-Al Si10 9,0-11,0 0,8 0,30 0,05 0,05 - - 0,10 0,20 - - - 0,05 0,15 Remainder
c
EN AW-4046 EN AW-Al Si10Mg 9,0-11,0 0,50 0,03 0,40 0,20-0,50 - - 0,10 0,15 - - 0,05 0,15 Remainder

c
EN AW-4047A EN AW-Al Si12(A) 11,0-13,0 0,6 0,30 0,15 0,10 - - 0,20 0,15 - - 0,05 0,15 Remainder
EN AW-4104 EN AW-Al Si10MgBi 9,0-10,5 0,8 0,25 0,10 1,0-2,0 - - 0,20 - - - 0,02-0,20 Bi 0,05 0,15 Remainder
EN AW-4343 EN AW-AI Si7,5 6,8-8,2 0,8 0,25 0,10 - - - 0,20 - - - - 0,05 0,15 Remainder
a
 "Others" includes listed elements for which no specific limit is shown as well as unlisted metallic elements. The producer may analyze samples for trace elements not specified in the registration or specification. However, such
analysis is not required and may not cover all metallic "Other" elements. Should any analysis by the producer or the purchaser establish that an "Others" element exceeds the limit of "Each" or that the aggregate of several "Others"
elements exceeds the limit of "Total", the material shall be considered non-conforming.
b
The sum of those "Others" metallic elements 0,010 % or more each, expressed to the second decimal place before determining the sum.
c
0,0003 max. Be for welding electrode, welding rod and filler wire only.


11

---------------------- Page: 13 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 5 — Aluminium alloys — 5 000 series — Al Mg
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
b
Numerical Chemical symbols Each min.
Total
EN AW-5005 EN AW-Al Mg1(B) 0,30 0,7 0,20 0,20 0,50-1,1 0,10 - 0,25 - - - - 0,05 0,15 Remainder
EN AW-5005A EN AW-Al Mg1(C) 0,30 0,45 0,05 0,15 0,7-1,1 0,10 - 0,20 - - - - 0,05 0,15 Remainder
EN AW-5006 EN AW-Al Mg1Mn0,5 0,40 0,80 0,10 0,40-0,8 0,8-1,3 0,10 - 0,25 0,10 - - - 0,05 0,15 Remainder
EN AW-5010 EN AW-Al Mg0,5Mn 0,40 0,7 0,25 0,10-0,30 0,20-0,6 0,15 - 0,30 0,10 - - - 0,05 0,15 Remainder
c
EN AW-5018 EN AW-Al Mg3Mn0,4 0,25 0,40 0,05 0,20-0,6 2,6-3,6 0,30 - 0,20 0,15 - - 0,05 0,15 Remainder
0,20-0,6 Mn+Cr
EN AW-5019 EN AW-Al Mg5 0,40 0,50 0,10 0,10-0,6 4,5-5,6 0,20 - 0,20 0,20 - - 0,10-0,6 Mn+Cr 0,05 0,15 Remainder
EN AW-5026 EN AW-Al Mg4,5MnSiFe 0,55-1,4 0,20-1,0 0,10-0,8 0,6-1,8 3,9-4,9 0,30 - 1,0 0,20 - - 0,30Zr 0,05 0,15 Remainder
EN AW-5040 EN AW-Al Mg1,5Mn 0,30 0,7 0,25 0,9-1,4 1,0-1,5 0,10-0,30 - 0,25 - - - - 0,05 0,15 Remainder
EN AW-5042 EN AW-Al Mg3,5Mn 0,20 0,35 0,15 0,20-0,50 3,0-4,0 0,10 - 0,25 0,10 - - - 0,05 0,15 Remainder
EN AW-5049 EN AW-Al Mg2Mn0,8 0,40 0,50 0,10 0,50-1,1 1,6-2,5 0,30 - 0,20 0,10 - - - 0,05 0,15 Remainder
EN AW-5050 EN AW-Al Mg1,5(C) 0,40 0,7 0,20 0,10 1,1-1,8 0,10 - 0,25 - - - - 0,05 0,15 Remainder
EN AW-5050A EN AW-Al Mg1,5(D) 0,40 0,7 0,20 0,30 1,1-1,8 0,10 - 0,25 - - - - 0,05 0,15 Remainder
EN AW-5051A EN AW-Al Mg2(B) 0,30 0,45 0,05 0,25 1,4-2,1 0,30 - 0,20 0,10 - - - 0,05 0,15 Remainder
EN AW-5052 EN AW-Al Mg2,5 0,25 0,40 0,10 0,10 2,2-2,8 0,15-0,35 - 0,10 - - - - 0,05 0,15 Remainder
EN AW-5058 EN AW-Al Mg5Pb1,5 0,40 0,50 0,10 0,20 4,5-5,6 0,10 - 0,20 0,20 - - 1,2-1,8 Pb 0,05 0,15 Remainder
EN AW-5059 EN-AW-Al Mg5,5MnZnZr 0,45 0,50 0,25 0,6-1,2 5,0-6,0 0,25 - 0,40-0,9 0,20 - - 0,05-0,25Zr 0,05 0,15 Remainder
EN AW-5070 EN AW-Al Mg4MnZn 0,25 0,40 0,25 0,40-0,8 3,5-4,5 0,30 - 0,40-0,8 0,15 - - - 0,05 0,15 Remainder
EN AW-5082 EN AW-Al Mg4,5 0,20 0,35 0,15 0,15 4,0-5,0 0,15 - 0,25 0,10 - - - 0,05 0,15 Remainder
EN AW-5083 EN AW-Al Mg4,5Mn0,7 0,40 0,40 0,10 0,40-1,0 4,0-4,9 0,05-0,25 - 0,25 0,15 - - - 0,05 0,15 Remainder
EN AW-5086 EN AW-Al Mg4 0,40 0,50 0,10 0,20-0,7 3,5-4,5 0,05-0,25 - 0,25 0,15 - - - 0,05 0,15 Remainder
c
EN AW-5087 EN AW-Al Mg4,5MnZr 0,25 0,40 0,05 0,7-1,1 4,5-5,2 0,05-0,25 - 0,25 0,15 - - 0,10-0,20 Zr 0,05 0,15 Remainder
EN AW-5088 EN AW-Al Mg5Mn0,4 0,20 0,10-0,35 0,25 0,20-0,50 4,7-5,5 0,15 - 0,20-0,40 - - - 0,15Zr 0,05 0,15 Remainder
EN AW-5110 EN AW-Al 99,85Mg0,5 0,08 0,08 - 0,03 0,30-0,6 - - 0,05 0,02 - - - 0,02 - Remainder

12

---------------------- Page: 14 ----------------------

SIST EN 573-3:2009
EN 573-3:2009 (E)
Table 5 — Aluminium alloys — 5 000 series — Al Mg (continued)
a
Alloy designation Others Aluminium
Si Fe Cu Mn Mg Cr Ni Zn Ti Ga V Remarks
b
Numerical Chemical symbols Each min.
Total
c
EN AW-5119 EN AW-Al Mg5(A) 0,25 0,40 0,05 0,20-0,6 4,5-5,6 0,30 - 0,20 0,15 - - 0,05 0,15 Remainder
0,20-0,6 Mn+Cr
e
EN AW-5119A EN-AW Al Mg5(B) 0,25 0,40 0,05 0,20-0,6 4,5-5,6 0,30 - 0,20 0,15  0,05 0,15 Remainder
0,20-0,6 Mn+Cr
EN AW-5149 EN AW-Al Mg2Mn0,8(A) 0,25 0,40 0,05 0,50-1,1 1,6-2,5 0,30 - 0,20 0,15 - - - 0,05 0,15 Remainder
c
EN AW-5154A EN AW-Al Mg3,5(A) 0,50 0,50 0,10 0,50 3,1-3,9 0,25 - 0,20 0,20 - - 0,05 0,15 Remainder
0,10-0,50 Mn+Cr
EN AW-5154B EN AW-Al Mg3,5Mn0,3 0,35 0,45 0,05 0,15-0,45 3,2-3,8 0,10 0,01 0,15 0,15 - - - 0,05 0,15 Remainder
-
EN AW-5182 EN AW-Al Mg4,5Mn0,4 0,20 0,35 0,15 0,20-0,50 4,0-5,0 0,10 - 0,25 0,10 - - 0,05 0,15 Remainder

c
EN AW-5183 EN AW-Al Mg4,5Mn0,7(A) 0,40 0,40 0,10 0,50-1,0 4,3-5,2 0,05-0,25 - 0,25 0,15 - - 0,05 0,15 Remainder
e
EN AW-5183A EN AW-Al Mg4,5Mn0,7(C) 0,40 0,40 0,10 0,50-1,0 4,3-5,2 0,05-0,25 - 0,25 0,15 - - 0,05 0,15 Remainder
EN AW-5186 EN AW-Al Mg4Mn0,4 0,40 0,45 0,25 0,20-0,50 3,8-4,8 0,15 - 0,40 0,15 - - 0,05 Zr 0,05 0,15 Remainder
e
EN AW-5187 EN AW-Al Mg4,5MnZr 0,25 0,40 0,05 0,7-1,1 4,5-5,2 0,05-0,25 - 0,25 0,15 - - 0,10-0,20 Zr 0,05 0,15 Remainder
EN AW-5210 EN AW-Al 99,9Mg0,5 0,06 0,04 - 0,03 0,35-0,6 - - 0,04 0,01 - - - 0,01 - Remainder
c
EN AW-5249 EN AW-Al Mg2Mn0,8Zr 0,25 0,40 0,05 0,50-1,1 1,6-2,5 0,30 - 0,20 0,15 - - 0,05 0,15 Remainder
0,10-0,20 Zr
EN AW-5251 EN AW-Al Mg2Mn0,3 0,40 0,50 0,15 0,10-0,50 1,7-2,4 0,15 - 0,15 0,15 - - - 0,05 0,15 Remainder
EN AW-5252 EN AW-Al Mg2,5(B) 0,08 0,10 0,10 0,10 2,2-2,8 - - 0,05 - - 0,05 - 0,03 0,10 Remainder
d
EN AW-5283A EN AW-Al Mg4,5Mn0,7(B) 0,30 0,30 0,03 0,50-1,0 4,5-5,1 0,05 0,03 0,10 0,03 - - 0,05 0,15 Remainder
0,05 Zr
EN AW-5305 EN AW-Al 99,85
...

Questions, Comments and Discussion

Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.