Standard Specification for Aluminum-Alloy Rolled Tread Plate

SCOPE
1.1 This specification covers aluminum-alloy rolled flat tread plate, mill-finish, with a raised pattern on one side, in the alloy, tempers, and thicknesses shown in Table 1 and Table 2.
1.2 Alloy and temper designation are in accordance with ANSI H35.1 [H35.1M]. The equivalent Unified Numbering System alloy designation are those of preceded by A9, which is A96061 for alloy 6061 and A93003 for Alloy 3003 in accordance with Practice E527.
1.3 For acceptance criteria for inclusion of new aluminum and aluminum alloys in this specification, see Annex A2.
1.4 The values stated in either inch-pound or SI units are to be regarded separately as standard. The SI units are shown either in brackets or in separate tables. The values stated in each system are not exact equivalents; therefore, each system must be used independently of the other. Combining values from the two systems will result in nonconformance with the specification.

General Information

Status
Historical
Publication Date
09-Oct-2002
Current Stage
Ref Project

Relations

Buy Standard

Technical specification
ASTM B632/B632M-02 - Standard Specification for Aluminum-Alloy Rolled Tread Plate
English language
7 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: B 632/B 632M – 02
Standard Specification for
1
Aluminum-Alloy Rolled Tread Plate
This standard is issued under the fixed designation B 632/B 632M; the number immediately following the designation indicates the year
of original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval.
A superscript epsilon (e) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the Department of Defense.
1. Scope * B 918 Practice for Heat Treatment of Wrought Aluminum
2
Alloys
1.1 This specification covers aluminum-alloy rolled flat
E 29 Practice for Using Significant Digits in Test Data to
tread plate, mill-finish, with a raised pattern on one side, in the
3
Determine Conformance with Specifications
alloy, tempers, and thicknesses shown in Table 1 and Table 2
E 34 Test Methods for ChemicalAnalysis ofAluminum and
[Table 3].
4
Aluminum-Base Alloys
1.2 Alloy and temper designation are in accordance with
E 55 Practice for SamplingWrought Nonferrous Metals and
ANSI H35.1 [H35.1M]. The equivalent Unified Numbering
4
Alloys for Determination of Chemical Composition
System alloy designation are those of Table 1 preceded byA9,
E 227 Test Method for Optical Emission Spectrometric
which isA96061 for alloy 6061 andA93003 forAlloy 3003 in
Analysis of Aluminum and Aluminum Alloys by the
accordance with Practice E 527.
4
Point-to-Plane Technique
1.3 For acceptance criteria for inclusion of new aluminum
E 290 Test Method for Bend Testing of Material for Duc-
and aluminum alloys in this specification, see Annex A2.
5
tility
1.4 The values stated in either inch-pound or SI units are to
6
E 527 Practice for Numbering Metals and Alloys (UNS)
be regarded separately as standard. The SI units are shown
E 607 Test Method for Optical Emission Spectrometric
either in brackets or in separate tables. The values stated in
Analysis of Aluminum and Aluminum Alloys by the
each system are not exact equivalents; therefore, each system
4
Point-to-Plane Technique, Nitrogen Atmosphere
must be used independently of the other. Combining values
E 716 Practices for Sampling Aluminum and Aluminum
from the two systems will result in nonconformance with the
4
Alloys for Spectrochemical Analysis
specification.
E 1251 Test Method for Optical Emission Spectrometric
2. Referenced Documents Analysis ofAluminum andAluminumAlloys by theArgon
Atmosphere, Point-to-Plane, Unipolar Self-Initiating Ca-
2.1 The following documents of the issue in effect on the
4
pacitor Discharge
date of material purchase form a part of this specification to the
2.3 ANSI Standards:
extent referenced herein:
H35.1 Alloy and Temper Designation Systems for Alumi-
2.2 ASTM Standards:
2
num
B 557 Test Methods of Tension Testing Wrought and Cast
2
H35.1M Alloy and Temper Designation Systems for Alu-
Aluminum- and Magnesium-Alloy Products
minum [Metric]
B 557M Test Methods ofTensionTestingWrought and Cast
2
H35.2 Dimensional Tolerances for Aluminum Mill Prod-
Aluminum- and Magnesium-Alloy Products [Metric]
2
ucts
B 660 Practices for Packaging/Packing of Aluminum and
2
H35.2M Dimensional Tolerances for Aluminum Mill Prod-
Magnesium Products
2
ucts [Metric]
B 666/B 666M Practice for Identification Marking of Alu-
2
minum and Magnesium Products
3. Terminology
B 881 Terminology Relating to Aluminum- and
2
3.1 Definitions: Refer to Terminology B 881 for definitions
Magnesium-Alloy Products
of product terms used in this specification.
1
This specification is under the jurisdiction of ASTM Committee B07 on Light
Metals and Alloys and is the direct responsibility of Subcommittee B07.03 on
3
Aluminum Alloy Wrought Products. Annual Book of ASTM Standards, Vol 14.02.
4
Current edition approved Oct. 10, 2002. Published December 2002. Originally Annual Book of ASTM Standards, Vol 03.05.
5
approved in 1978. Last previous edition approved in 2001 as B 632/B 632M–01. Annual Book of ASTM Standards, Vol 03.01.
2 6
Annual Book of ASTM Standards, Vol 02.02. Annual Book of ASTM Standards, Vol 01.01.
*A Summary of Changes section appears at the end of this standard.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.
1

---------------------- Page: 1 ----------------------
B 632/B 632M – 02
A,B,C
TABLE 1 Chemical Composition Limits
D
Alloy Silicon Iron Copper Manganese Magnesium Chromium Zinc Titanium Other Elements Aluminum
E
Each Total
3003 0.6 0.7 0.05-0.20 1.0-1.5 - - - - - - 0.10 - - - 0.05 0.15 Remainder
6061 0.40-0.8 0.7 0.15-0.40 0.15 0.8-1.2 0.04-0.35 0.25 0.15 0.05 0.15 Remainder
A
Limits in weight percent maximum unless shown as a range or minimum
B
Analysis shall be made for the elements for which limits are shown in this table.
C
For purposes of det
...

Questions, Comments and Discussion