Abstract

This document specifies a method of tensile testing of metallic materials at temperatures higher than room temperature.

Status
Published
Publication Date
11-Aug-2026
Current Stage
6060 - Definitive text made available (DAV) - Publishing
Start Date
12-Aug-2026
Due Date
12-Aug-2026
Completion Date
12-Aug-2026

Buy Documents

Standard

EN ISO 6892-2:2026

English language (28 pages)
Preview
Preview
e-Library read for
×1 day

EN ISO 6892-2:2026 is a European Standard published by CEN that adopts ISO 6892-2:2026 without modification. It specifies a method of tensile testing of metallic materials at temperatures higher than room temperature. The standard is intended for laboratories, manufacturers, and users who need elevated-temperature tensile properties for metallic materials.

What does EN ISO 6892-2:2026 specify?

EN ISO 6892-2:2026 specifies the test method for tensile testing of metallic materials at elevated temperature. It defines how to prepare the test piece, set up the equipment, choose the test rate, and report the results so that the test can be repeated and compared in practice.

The document is organized into clauses on scope, normative references, terms and definitions, symbols, principle, test piece, original cross-sectional area, marking the gauge length, apparatus, test conditions, determination of properties, test report, measurement uncertainty, figures, and annexes.

AnnexWhat it covers
Annex AAdditional information on test piece geometries used for testing at elevated temperature
Annex BMeasurement uncertainty

What are the key requirements of EN ISO 6892-2:2026?

EN ISO 6892-2:2026 requires tensile testing to be carried out above room temperature, with the test temperature higher than 35 °C. In practice, that means the test is for hot-condition material behavior, not ambient testing.

Test pieces, gauge length, and basic setup

The test piece requirements, original cross-sectional area, and marking of the original gauge length follow ISO 6892-1. This keeps the elevated-temperature method aligned with the room-temperature part of the tensile test series and helps users apply the same specimen philosophy across both methods.

Clause 6 notes that Annex A gives additional example geometries. Annex A is useful when you need a specimen shape that can be gripped reliably while heated.

Apparatus and calibration

Clause 9 requires the force-measuring system to be calibrated to ISO 7500-1, class 1 or better. The extensometer used for proof strength properties shall meet ISO 9513, class 1 or better in the relevant range, while class 2 may be used for properties with higher extension. For the reader, this means the machine and extensometer must be suitable for accurate force and extension measurement before any test results can be trusted.

The heating system must be able to bring the test piece to the specified temperature. The temperature control rules are strict because elevated-temperature tensile properties are sensitive to small temperature differences. Clause 9 also requires temperature measurement with a resolution of 1 °C or better, periodic calibration of the measuring chain, and direct measurement on the test piece.

Temperature control and soaking time

The document sets permitted deviations between the specified temperature and the indicated temperature, together with maximum temperature differences along the parallel length of the test piece. The limits are given in Table 2, and the laboratory has to verify them by the end of the soaking time and before loading starts.

Clause 10 requires the test piece to be held at the specified temperature for at least 10 minutes before loading. This matters because the full cross-section may need longer to stabilize, especially for thicker or less responsive specimens.

Force zero, gripping, and extensometer setting

Clause 10.1 requires the force-measuring system to be zeroed after the machine is assembled but before the test piece is placed in the grips, and it must not be changed during the test. In practice, this reduces the influence of gripping and fixture weight on the measured force.

Clause 10.2 requires gripping in accordance with ISO 6892-1 and says the method used to establish the extensometer gauge length shall be documented. The document gives three gauge-length approaches at test temperature - Method 1, Method 2 a, Method 2 b, and Method 2 c. That choice matters because thermal expansion can affect the calculated extension values.

Test rates: Method A and Method B

EN ISO 6892-2:2026 provides two rate-control approaches. Method A uses strain-rate control with narrow tolerances of ±20 percent and is intended to reduce variation during the part of the test where strain-rate-sensitive properties are determined. Method B uses expanded, traditional strain-rate ranges.

For Method A, the document gives specified strain-rate ranges for determining upper yield strength or proof strength properties, lower yield strength and percentage yield point extension, and tensile strength-related properties such as tensile strength, percentage elongation after fracture, and percentage reduction of area. If the test equipment cannot directly control strain rate, crosshead displacement control is used instead.

For Method B, the document gives the initial strain-rate range for yield or proof strength and a separate range for tensile strength. If yield strength and tensile strength are determined on the same specimen, the change in rate must be smooth and avoid overshoot.

Choice of method and reporting

Clause 10.5 allows the laboratory to choose Method A or Method B, unless otherwise specified or agreed. Clause 10.6 gives the abbreviated notation for reporting the selected control mode and rate combination. That helps laboratories record exactly how the test was run, which is important when comparing results across sites or with product specifications.

Clause 12 requires the report to identify the standard, the specimen, the material if known, the specimen type, sampling location and direction if known, the control mode and rates when relevant, soaking time, test temperature, extensometer gauge-length method, deviations, results, and test date.

Measurement uncertainty

Clause 13 points to ISO 6892-1 and Annex B for measurement uncertainty. Annex B shows that temperature and strain-rate effects can influence all listed tensile properties at elevated temperature. For the user, this means uncertainty estimates need to include not only the machine and extensometer but also the sensitivity of the material to temperature and loading rate.

What terms does EN ISO 6892-2:2026 define?

  • Original gauge length - the distance between the gauge length marks on the test piece measured at room temperature before heating and before force is applied.
  • Percentage elongation after fracture (A) - the permanent elongation of the gauge length after fracture, expressed as a percentage of the original gauge length.
  • Extensometer gauge length - the length of the parallel portion used for extension measurement by an extensometer.
  • Extension - the increase in extensometer gauge length at a given moment during the test.
  • Percentage reduction of area (Z) - the maximum change in cross-sectional area that occurs during the test, expressed as a percentage of the original area.
  • Stress (R) - the force at any moment during the test divided by the original cross-sectional area of the test piece.
  • Soaking time (t_s) - the time used to stabilize the temperature of the test piece before mechanical loading starts.

Who uses EN ISO 6892-2:2026?

EN ISO 6892-2:2026 is used by mechanical testing laboratories, materials engineers, quality managers, and purchasers who need elevated-temperature tensile data. It is relevant in metals production and qualification work where the behavior of steel and other metallic materials at temperature has to be measured consistently.

The standard is also used when comparing elevated-temperature results with room-temperature tensile properties at the same strain rate, or when a product standard asks for proof strength, yield strength, tensile strength, elongation, or reduction of area at temperature. Annex A shows applications to sheets, strips, flats, wires, bars, sections, and tubes.

What changed in EN ISO 6892-2:2026 from the previous edition?

EN ISO 6892-2:2026 supersedes EN ISO 6892-2:2018. The foreword states that this third edition is technically revised.

The changes listed include:

  • revision of Clause 9.3
  • wording changes in 10.3
  • wording changes in 10.4
  • revision of Clause 12
  • wording changes in Annex A
  • updated references, especially to ISO 6892-1, specific clauses, figures and annexes
  • editorial modifications

Which standards are used with EN ISO 6892-2:2026?

  • ISO 6892-1:2019 - provides the room-temperature tensile-test framework that EN ISO 6892-2 builds on, including specimen rules, symbols, property calculation, uncertainty treatment, and several referenced figures and annexes.
  • ISO 7500-1 - provides calibration and verification requirements for the force-measuring system of the testing machine.
  • ISO 9513 - provides calibration requirements for extensometer systems used in uniaxial testing.

What does the EN ISO 6892-2:2026 document contain?

EN ISO 6892-2:2026 contains a strain-rate control method, a traditional strain-rate-range method, and the reporting format for each. It also contains the temperature-control rules, including permitted deviations, sensor placement, and soaking time, which are central to elevated-temperature testing.

The document includes Table 1 for symbols, Table 2 for temperature tolerances, Figure 1 for the strain-rate sequence used in Method A, Annex A with specimen geometry examples and figures, and Annex B with uncertainty guidance, a contributor table, and example stress-strain figures. Those parts are used for test setup, laboratory practice, and interpreting results for design, quality control, and material qualification.

Relations

Effective Date
04-Oct-2023
Effective Date
07-Oct-2026
Effective Date
07-Oct-2026
Effective Date
07-Oct-2026
Effective Date
04-Nov-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026
Effective Date
19-Aug-2026

Buy Documents

Standard

EN ISO 6892-2:2026

English language (28 pages)
Preview
Preview
e-Library read for
×1 day

Get Certified

Connect with accredited certification bodies for this standard

Element Materials Technology

Materials testing and product certification.

UKAS United Kingdom Verified

Inštitut za kovinske materiale in tehnologije

Institute of Metals and Technology. Materials testing, metallurgical analysis, NDT.

SA Slovenia Verified

Sponsored listings

Frequently Asked Questions

EN ISO 6892-2:2026 is a standard published by the European Committee for Standardization (CEN). Its full title is "Metallic materials - Tensile testing - Part 2: Method of test at elevated temperature (ISO 6892-2:2026)". This standard covers: This document specifies a method of tensile testing of metallic materials at temperatures higher than room temperature.

This document specifies a method of tensile testing of metallic materials at temperatures higher than room temperature.

EN ISO 6892-2:2026 is classified under the following ICS (International Classification for Standards) categories: 77.040.10 - Mechanical testing of metals. The ICS classification helps identify the subject area and facilitates finding related standards.

EN ISO 6892-2:2026 has the following relationships with other standards: It is inter standard links to EN ISO 6892-2:2018, ISO 9513:2012, ISO 6892-1:2019, ISO 7500-1:2018, EN 10253-3:2026, EN 4800-006:2010, EN 15566:2016, EN 4700-003:2010, EN 4800-007:2010, EN 10088-2:2014, EN 4700-002:2010, EN 10216-3:2002, EN 4800-005:2010, EN 1999-1-1:2007, EN 10217-5:2002. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.

EN ISO 6892-2:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)

Contents

  • Introduction
  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 3.1 original gauge length
  • 3.2 percentage elongation after fracture
  • 3.3 extensometer gauge length
  • 3.4 extension
  • 3.5 percentage extension
  • 3.6 percentage reduction of area
  • 3.7 stress
  • 3.8 soaking time
  • 4 Symbols
  • 5 Principle
  • 6 Test piece
  • 7 Determination of original cross-sectional area (S )
  • 8 Marking the original gauge length (L )
  • 9 Apparatus
  • 10 Test conditions
  • 10.1 Setting the force zero point
  • 10.2 Gripping of the test piece, fixing of the extensometer and heating of the test piece, not
  • 10.3 Testing rate based on strain rate control (Method A)
  • 10.4 Method of testing with expanded strain rate ranges (Method B)
  • 10.5 Choice of the method and rates
  • 10.6 Documentation of the chosen testing conditions
  • 11 Determination or calculation of the properties
  • 12 Test report
  • 13 Measurement uncertainty
  • 14 Figures
  • 15 Annexes
  • Annex A
  • Annex B
  • Bibliography

Introduction

In this document, two methods of testing speeds are described. The first, Method A, is based on strain rates (including crosshead separation rate) with narrow tolerances (±20 %) and the second, Method B, is based on conventional strain rate ranges and tolerances (strain rates from former editions). Method A is intended to minimize the variation of the test rates during the moment when strain rate-sensitive parameters are determined and to minimize the measurement uncertainty of the test results. The influence of the testing speed on the mechanical properties, determined by the tensile test, is normally greater at an elevated temperature than at room temperature.

Traditionally, mechanical properties determined by tensile tests at elevated temperatures have been determined at a slower strain or stressing rate than at room temperature. This document recommends the use of slow strain rates but, in addition, higher strain rates are permitted for particular applications, such as comparison with room temperature properties at the same strain rate.

SIST EN ISO 6892-2:2026

SIST EN ISO 6892-2:2026 International Standard ISO 6892-2:2026(en) Metallic materials — Tensile testing — Part 2:

Method of test at elevated temperature WARNING — This document calls for the use of either substances or procedures, or both, that can be injurious to health if adequate safety measures are not taken. This document does not address any health hazards, safety or environmental matters associated with its use. It is the responsibility of the user of this document to establish appropriate health, safety and environmentally acceptable practices.

1 Scope

This document specifies a method of tensile testing of metallic materials at temperatures higher than room temperature.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 6892-1:2019, Metallic materials — Tensile testing — Part 1: Method of test at room temperature ISO 7500-1, Metallic materials — Calibration and verification of static uniaxial testing machines — Part 1:

Tension/compression testing machines — Calibration and verification of the force-measuring system ISO 9513, Metallic materials — Calibration of extensometer systems used in uniaxial testing

3 Terms and definitions

For the purposes of this document, the terms and definitions given in ISO 6892-1 and the following apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:

  • ISO Online browsing platform: available at https:// www .iso .org/ obp
  • IEC Electropedia: available at https:// www .electropedia .org/

3.1 original gauge length

L o distance between gauge length marks on the test piece measured at room temperature before heating of the test piece and before application of force

3.2 percentage elongation after fracture

A permanent elongation at room temperature of the gauge length after fracture (L − L ) u o Note 1 to entry: A is expressed as a percentage of the original gauge length (L ) (3.1). o Note 2 to entry: For further details, see ISO 6892-1.

SIST EN ISO 6892-2:2026 ISO 6892-2:2026(en)

3.3 extensometer gauge length

L e length within the parallel portion of the test piece used for the measurement of extension (3.4) by means of an extensometer

3.4 extension

increase in the extensometer gauge length (L ) (3.3) at a given moment during the test e

3.5 percentage extension

extension (3.4) expressed as a percentage of the extensometer gauge length (L ) (3.3) e

3.6 percentage reduction of area

Z maximum change in cross-sectional area which has occurred during the test (S − S ) o u Note 1 to entry: Z is expressed as a percentage of the original cross-sectional area (S ), where S and S are calculated o o u from the dimensions at room temperature.

3.7 stress

R force at any moment during the test divided by the original cross-sectional area (S ) of the test piece o Note 1 to entry: All stresses referred to in this document are engineering stresses, calculated using the cross-sectional area of the test piece derived from dimensions measured at room temperature.

3.8 soaking time

t s time taken to stabilize the temperature of the test piece prior to mechanical loading

4 Symbols

ISO 6892-1 provides an extensive listing of symbols and their related designations. The additional symbols used in this document are given in Table 1. Table 1 — Symbols and designations Symbol Designation Unit T specified temperature or nominal temperature at which the test should be performed °C T indicated temperature or measured temperature on the surface of the parallel length of the test piece °C

t soaking time min s

5 Principle

The test involves straining a test piece by tensile force for the determination of one or more of the mechanical properties defined in Clause 3.

The test shall be carried out at a temperature higher than 35 °C, which means at temperatures higher than room temperature as specified in ISO 6892-1.

SIST EN ISO 6892-2:2026 ISO 6892-2:2026(en)

6 Test piece

The requirements of the test pieces shall be in accordance with ISO 6892-1. NOTE Additional examples of test pieces are given in Annex A.

7 Determination of original cross-sectional area (S )

o The requirements concerning determination of the original cross-sectional area shall be in accordance with ISO 6892-1.

NOTE S is calculated from measurements taken at room temperature. o

8 Marking the original gauge length (L )

o The requirements concerning the marking of the original gauge length shall be in accordance with ISO 6892-1.

9 Apparatus

9.1 Force-measuring system.

The force-measuring system of the testing machine shall be calibrated in accordance with ISO 7500-1, class 1, or better.

9.2 Extensometer.

For the determination of proof strength (plastic or total extension), the used extensometer shall be in accordance with ISO 9513, class 1 or better, in the relevant range. For other properties (with higher extension), an ISO 9513 class 2 extensometer in the relevant range may be used. The extensometer gauge length shall be not less than 10 mm and shall correspond to the central portion of the parallel length.

Any part of the extensometer projecting beyond the furnace shall be designed or protected from fluctuations in air flow and room temperature, to have only a minimal effect on the readings. It is advisable to maintain reasonable stability of the temperature and speed of the air surrounding the testing machine. 9.3 Heating device system.

9.3.1 The heating device system consists from several parts:

  • heating device (e.g. furnace or oven);
  • temperature controller;
  • temperature measuring system.

The heating device system for the test piece shall be capable of heating the test piece to the specified temperature, T.

9.3.2 Permitted deviations of temperature.

The indicated temperatures, T , are the temperatures measured on the surface of the parallel length of the

test piece with corrections applied for any known systematic errors (verified bias). The permitted deviations between the specified temperature, T, and the indicated temperatures, T , and the

maximum permissible temperature difference within the entire parallel length of the test piece are given in

SIST EN ISO 6892-2:2026 ISO 6892-2:2026(en) Table 2. The laboratory shall verify that the permitted deviations are fulfilled at the end of the soaking time to the start of the test. The measured temperature should be recorded during the complete test to identify deviations.

For specified temperatures greater than 1 100 °C, the permitted deviations shall be defined by previous agreement between the parties concerned.

Table 2 — Permitted deviations between T and T and maximum permissible temperature

differences along the test piece Maximum permissible temperature Specified temperature Permitted deviation between T and T

differences along the test piece T °C °C °C T ≤ 600 ±3 3 600 < T ≤ 800 ±4 4 800 < T ≤ 1 000 ±5 5 1 000 < T ≤ 1 100 ±6 6 9.3.3 Measurement of temperature.

When the parallel length is less than 50 mm, one temperature sensor shall measure the temperature at each end of the parallel length directly. When the parallel length is equal to or greater than 50 mm, a third temperature sensor shall measure near the centre of the parallel length. This number may be reduced if the general arrangement of the furnace and the test piece is such that, from experience, it is known that the variation in temperature of the test piece does not exceed the permitted deviation specified in 9.3.1. However, at least one sensor shall be measuring the test piece temperature directly.

Temperature sensor junctions shall make good thermal contact with the surface of the test piece and be suitably screened from direct radiation from the furnace wall. 9.3.4 Temperature-measuring system.

The temperature-measuring system shall have a resolution equal to or better than 1 °C. The temperature-measuring system (sensor, cables, indicating device and reference junction) should be calibrated over the working range at intervals of 12 months, but the intervals shall not exceed 13 months. This should be done with the complete measurement chain as a single unit. Verify that the temperaturemeasuring system is able to fulfil the requirements given in Table 2. Bias shall be recorded on the verification report. The components of the temperature-measuring system shall be verified by methods traceable to the international unit (SI unit) of temperature.

NOTE The temperature-measuring system includes all components of the measuring chain (sensor, cables, indicating device and reference junction).

10 Test conditions

10.1 Setting the force zero point

The force-measuring system shall be set to zero after the testing equipment has been assembled but before the test piece is actually placed in the gripping jaws. Once the force zero point has been set, the forcemeasuring system shall not be changed in any way during the test. NOTE The use of this method ensures that the weight of the gripping system is compensated in the force measurement and that any force resulting from the clamping operation has a significantly reduced influence to the force zero point.

SIST EN ISO 6892-2:2026 ISO 6892-2:2026(en)

10.2 Gripping of the test piece, fixing of the extensometer and heating of the test piece, not

necessarily in the following sequence

10.2.1 Method of gripping

The requirements concerning the method of gripping shall be in accordance with ISO 6892-1:2019, 10.2. NOTE Maintaining a very small tensile load (e.g. test machine in force control) during heating period and soaking time can prevent possible compressive stresses due to thermal expansion.

10.2.2 Fixing of the extensometer and establishing the gauge length
10.2.2.1 General

Different methods of establishing the extensometer gauge length are used in practice. This can lead to minor differences in the test results. The method used shall be documented in the test report. Once the extensometer reading is set to zero at L , this should not be adjusted to account for such things as e thermal expansion.

...