ISO 23146:2012 specifies a method for the determination of the fracture toughness of advanced technical ceramics. The procedure makes use of single-edge V-notched bars, which are loaded in four-point bending until failure. It is applicable to monolithic ceramics with a grain size or major microstructural feature size larger than about 1 µm. The use of ISO 23146:2012 for yttria tetragonal zirconia polycrystal material (Y-TZP) is not recommended. The method might also be unsuitable for some other very tough or soft ceramics in which a sharp crack does not form at the root of the V-notch.
- Status
- Published
- Publication Date
- 12-Dec-2012
- Technical Committee
- ISO/TC 206 - Fine ceramics
- Drafting Committee
- ISO/TC 206 - Fine ceramics
- Current Stage
- 9092 - International Standard to be revised
- Start Date
- 13-Nov-2023
- Completion Date
- 29-Aug-2026
Buy Documents
ISO 23146:2012 - Fine ceramics (advanced ceramics, advanced technical ceramics) -- Test methods for fracture toughness of monolithic ceramics -- Single-edge V-notch beam (SEVNB) method
ISO 23146:2012 - Fine ceramics (advanced ceramics, advanced technical ceramics) — Test methods for fracture toughness of monolithic ceramics — Single-edge V-notch beam (SEVNB) method/13/2012
ISO 23146:2012 - Céramiques techniques -- Méthodes d'essai pour la détermination de la ténacité a la rupture des céramiques monolithiques -- Méthode sur éprouvette a entaille en V sur une seule face (Méthode SEVNB)
ISO 23146:2012 - Céramiques techniques — Méthodes d'essai pour la détermination de la ténacité à la rupture des céramiques monolithiques — Méthode sur éprouvette à entaille en V sur une seule face (Méthode SEVNB)/20/2013
Overview
ISO 23146:2012 specifies the SEVNB (single-edge V‑notch beam) method for determining the fracture toughness of monolithic advanced technical ceramics (fine ceramics). The method uses rectangular bar specimens with a machined V‑notch that are loaded in four‑point (or optionally three‑point) bending until failure. It is intended for materials with grain size or major microstructural features larger than about 1 µm. The standard notes limitations: it is not recommended for Y‑TZP (yttria‑stabilized tetragonal zirconia polycrystal) and may be unsuitable for very tough or soft ceramics where a sharp crack does not form at the notch root.
Key Topics
- Test principle: Prepare a sharp V‑notch (razor blade + diamond paste reciprocating honing) and fracture bars in bending to derive fracture toughness.
- Specimen requirements: Rectangular bars (typical cross section W = 4.0 ± 0.2 mm, B = 3.0 ± 0.2 mm) with length > 45 mm (1/4‑point) or > 35 mm (1/3‑point). At least seven pieces are prepared (five for test, two as dummies).
- Notch preparation: Notch‑root radii typically 1 µm–20 µm; provisional criterion: notch radius ≤ ~2× average grain size. Starter notch made by diamond saw (~0.5 mm deep) then honed to a sharp tip.
- Apparatus essentials: Razor blades, metallographic diamond paste (≈1–3 µm), lubricants, four‑point flexural fixture (outer rollers 5.0 mm ± 0.2 mm diameter), calibrated micrometer (0.002 mm), optical microscope (50×–500×), ultrasonic cleaner, and mechanical testing machine per ISO 7500‑1.
- Measurement & calculation: Record fracture load in flexure, measure notch depth and notch‑root geometry post‑fracture, calculate fracture toughness per procedures in the standard. Annexes address machine honing, interlaboratory evaluation, and corrections for effective crack length.
Applications
- Materials R&D: Comparing fracture toughness of candidate ceramics and processing routes.
- Quality control: Routine batch testing for brittle ceramic components.
- Failure analysis: Quantifying toughness in fractured parts and correlating to microstructure.
- Standards compliance & procurement: Specifying and verifying mechanical performance of advanced ceramics supplied for aerospace, medical, electronics, and engineering applications. Typical users include ceramic manufacturers, independent testing laboratories, research institutes, and design engineers working with fine/advanced ceramics.
Related Standards (if applicable)
- ISO 15732 - SEPB (single‑edge precracked beam) fracture toughness method
- ISO 18756 - Surface crack in flexure method
- ISO 24370 - Chevron notch method
- ISO 14704 - Flexural strength of monolithic ceramics
- ISO 7500‑1, ISO 3611 - measurement and machine verification references
Keywords: ISO 23146, SEVNB method, fracture toughness, advanced ceramics, fine ceramics, monolithic ceramics, ceramic testing standards.
Relations
- Effective Date
- 19-May-2012
Buy Documents
ISO 23146:2012 - Fine ceramics (advanced ceramics, advanced technical ceramics) -- Test methods for fracture toughness of monolithic ceramics -- Single-edge V-notch beam (SEVNB) method
ISO 23146:2012 - Fine ceramics (advanced ceramics, advanced technical ceramics) — Test methods for fracture toughness of monolithic ceramics — Single-edge V-notch beam (SEVNB) method/13/2012
ISO 23146:2012 - Céramiques techniques -- Méthodes d'essai pour la détermination de la ténacité a la rupture des céramiques monolithiques -- Méthode sur éprouvette a entaille en V sur une seule face (Méthode SEVNB)
ISO 23146:2012 - Céramiques techniques — Méthodes d'essai pour la détermination de la ténacité à la rupture des céramiques monolithiques — Méthode sur éprouvette à entaille en V sur une seule face (Méthode SEVNB)/20/2013
Frequently Asked Questions
ISO 23146:2012 is a standard published by the International Organization for Standardization (ISO). Its full title is "Fine ceramics (advanced ceramics, advanced technical ceramics) — Test methods for fracture toughness of monolithic ceramics — Single-edge V-notch beam (SEVNB) method". This standard covers: ISO 23146:2012 specifies a method for the determination of the fracture toughness of advanced technical ceramics. The procedure makes use of single-edge V-notched bars, which are loaded in four-point bending until failure. It is applicable to monolithic ceramics with a grain size or major microstructural feature size larger than about 1 µm. The use of ISO 23146:2012 for yttria tetragonal zirconia polycrystal material (Y-TZP) is not recommended. The method might also be unsuitable for some other very tough or soft ceramics in which a sharp crack does not form at the root of the V-notch.
ISO 23146:2012 specifies a method for the determination of the fracture toughness of advanced technical ceramics. The procedure makes use of single-edge V-notched bars, which are loaded in four-point bending until failure. It is applicable to monolithic ceramics with a grain size or major microstructural feature size larger than about 1 µm. The use of ISO 23146:2012 for yttria tetragonal zirconia polycrystal material (Y-TZP) is not recommended. The method might also be unsuitable for some other very tough or soft ceramics in which a sharp crack does not form at the root of the V-notch.
ISO 23146:2012 is classified under the following ICS (International Classification for Standards) categories: 81.060.30 - Advanced ceramics. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO 23146:2012 has the following relationships with other standards: It is inter standard links to ISO 23146:2008. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.
ISO 23146:2012 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
INTERNATIONAL ISO
STANDARD 23146
Second edition
2012-12-15
Fine ceramics (advanced ceramics,
advanced technical ceramics) — Test
methods for fracture toughness of
monolithic ceramics — Single-edge
V-notch beam (SEVNB) method
Céramiques techniques — Méthodes d’essai pour la détermination de
la ténacité à la rupture des céramiques monolithiques — Méthode sur
éprouvette à entaille en V sur une seule face (Méthode SEVNB)
Reference number
©
ISO 2012
© ISO 2012
All rights reserved. Unless otherwise specified, no part of this publication may be reproduced or utilized in any form or by any
means, electronic or mechanical, including photocopying and microfilm, without permission in writing from either ISO at the
address below or ISO’s member body in the country of the requester.
ISO copyright office
Case postale 56 • CH-1211 Geneva 20
Tel. + 41 22 749 01 11
Fax + 41 22 749 09 47
E-mail copyright@iso.org
Web www.iso.org
Published in Switzerland
ii © ISO 2012 – All rights reserved
Contents Page
Foreword .iv
1 Scope . 1
2 Normative references . 1
3 Terms and definitions . 1
4 Principle . 1
5 Apparatus . 2
6 Test piece preparation . 3
6.1 Number of test pieces . 3
6.2 Test-piece dimensions . 4
6.3 Preparing the V-notch by hand . 4
6.4 Preparing the V-notches by machine (optional) . 7
6.5 Determination of notch-root radius . 7
7 Test procedure . 8
7.1 Dimensions of test piece . 8
7.2 Flexural-strength test . 8
7.3 Measurement of notch depth . 9
7.4 Calculation of fracture toughness . 9
8 Precision and bias .11
9 Test report .11
Annex A (informative) Notch honing by machine .12
Annex B (informative) Interlaboratory evaluation of the SEVNB fracture toughness
test procedures .14
Annex C (informative) Corrections for effective crack length greater than notch depth .16
Bibliography .17
Foreword
ISO (the International Organization for Standardization) is a worldwide federation of national standards
bodies (ISO member bodies). The work of preparing International Standards is normally carried out
through ISO technical committees. Each member body interested in a subject for which a technical
committee has been established has the right to be represented on that committee. International
organizations, governmental and non-governmental, in liaison with ISO, also take part in the work.
ISO collaborates closely with the International Electrotechnical Commission (IEC) on all matters of
electrotechnical standardization.
International Standards are drafted in accordance with the rules given in the ISO/IEC Directives, Part 2.
The main task of technical committees is to prepare International Standards. Draft International
Standards adopted by the technical committees are circulated to the member bodies for voting.
Publication as an International Standard requires approval by at least 75 % of the member bodies
casting a vote.
Attention is drawn to the possibility that some of the elements of this document may be the subject of
patent rights. ISO shall not be held responsible for identifying any or all such patent rights.
ISO 23146 was prepared by Technical Committee ISO/TC 206, Fine ceramics.
This second edition cancels and replaces the first edition (ISO 23146:2008), of which it constitutes a
minor revision.
iv © ISO 2012 – All rights reserved
INTERNATIONAL STANDARD ISO 23146:2012(E)
Fine ceramics (advanced ceramics, advanced technical
ceramics) — Test methods for fracture toughness of
monolithic ceramics — Single-edge V-notch beam
(SEVNB) method
1 Scope
This International Standard specifies a method for the determination of the fracture toughness of
advanced technical ceramics. The procedure makes use of single-edge V-notched bars, which are loaded
in four-point bending until failure. It is applicable to monolithic ceramics with a grain size or major
microstructural feature size larger than about 1 µm.
The use of this International Standard for yttria tetragonal zirconia polycrystal material (Y-TZP) is not
recommended. The method might also be unsuitable for some other very tough or soft ceramics in which
a sharp crack does not form at the root of the V-notch.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated
references, only the edition cited applies. For undated references, the latest edition of the referenced
document (including any amendments) applies.
ISO 3611, Geometrical product specifications (GPS) — Dimensional measuring instruments; Micrometers
for external measurements — Design and metrological characteristics
ISO 7500-1, Metallic materials — Verification of static uniaxial testing machines — Part 1: Tension/compression
testing machines — Verification and calibration of the force-measuring system
ISO 14704, Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for flexural
strength of monolithic ceramics at room temperature
ISO 15732, Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for fracture
toughness of monolithic ceramics at room temperature by single edge precracked beam (SEPB) method
3 Terms and definitions
For the purposes of this document, the terms and definitions given in ISO 15732 apply.
4 Principle
This method of conducting a fracture toughness test is based on the preparation and fracture of bar
test pieces in which a sharp-tipped notch is machined. Using the technique of a reciprocating razor
blade and diamond paste, a narrow notch can be honed into a test piece using either a manual method
or a simple machine. Under well-controlled conditions, a notch-tip radius in the range of 1 µm to 20 µm
can be prepared depending on the grain size of the test material. For many materials, this is a close
approximation to a sharp crack, and the method has been found to give fracture toughness values
very close to those of other methods such as the single-edge precracked beam method (ISO 15732) or
the surface crack in flexure method (ISO 18756), provided that a sharp crack forms at the root of the
notch either during its preparation or during the subsequent fracture sequence. The method has the
advantage of simplicity of notch production compared with using a sharp-tipped diamond saw or a
diamond impregnated wire in which the tip radius is normally greater than 50 µm. The method is often
easier to undertake compared with other methods of precracking and is applicable to a wider range of
materials outside the scope of these methods.
The method has been extensively researched (see the Bibliography) and has been evaluated in an ESIS
(European Structural Integrity Society)/VAMAS (Versailles Agreement on Advanced Materials and
Standards) round robin, the results of which are summarized in Annex B. This recommended practice is
based upon the ESIS/VAMAS SEVNB round robin.
The method may have some limitations for materials with grain sizes of less than 1 µm, for which
the assumption that the notch approximates to a sharp crack may not be valid (see Annex C). Users
should strive to minimize the notch-root radius in the test pieces. This International Standard places a
provisional criterion that the notch-root radius should be similar to or less than twice the average grain
size of the material.
The method is complementary to other methods of measuring fracture toughness described in ISO 15732
(single-edge precracked beam method), ISO 18756 (surface crack in flexure method), and ISO 24370
(chevron notch method); see the Bibliography.
5 Apparatus
5.1 Ordinary razor blades, preferably with a support along one edge but alternatively inserted in a
suitable holder.
NOTE 1 Razor blades thinner than about 0,2 mm are not ideal for this task unless stiffened by a support, such
as by gluing or screwing between two steel plates, leaving only about 2 mm of edge showing. A razor blade with a
tip angle of 30° or smaller is ideal.
NOTE 2 Although it is possible to machine the notches entirely by hand, the use of a simple device in which the
test pieces are mounted and in which a razor blade primed with diamond paste is moved in a reciprocating motion
across the mounted test pieces has a distinct advantage, as this provides controlled loading and directional
stability to the razor blade, and sharper notches are produced. An example is shown in Annex A.
5.2 Metallographic diamond paste, in a viscous organic carrier and of fine grain size, typically
1 µm to 3 µm.
5.3 Lubricant, a light lubricating oil for lubricating the razor blade, e.g. clock oil.
5.4 Test piece support, consisting of a flat plate or other suitable device for mounting test pieces
during notch honing.
5.5 Flexural-strength test fixture, preferably a four-point flexural-strength test fixture operating in
accordance with the requirements of ISO 14704, i.e. either 1/4-point flexure (preferred) or 1/3-point
flexure. Alternatively, a three-point flexural-strength test jig may also be used, but the alignment of the
V-notch with the central loading roller is more critical.
The test piece is supported on two bearing edges perpendicular to its length. The outer-support bearing
edges shall be parallel rollers of diameter 5,0 mm ± 0,2 mm and shall be capable of rolling outward on
flat support surfaces. Preferably, one of the rollers shall additionally be capable of rotating about an axis
parallel to the length of the test piece such that torsional loading is minimised. The two rollers shall
be positioned initially with their centres 40,0 mm ± 0,5 mm (1/4-point flexure) or 30 mm ± 0,5 mm
(1/3-point flexure) apart with their axes parallel to within 1°. The separation of the centres of the rollers
in their starting positions shall be measured to the nearest 0,1 mm with a travelling microscope. The
rollers shall be made from hardened steel or other hard material with a hardness greater than 40 HRC
(Rockwell C-scale). The rollers shall have a smooth burr-free surface finish with roughness less than
0,5 µm Ra and shall have a diameter uniform to ± 0,02 mm.
For four-point flexure, the two loading rollers are located at the 1/4-points (or 1/3-points), with an inner
span of 20 mm ± 0,2 mm (or 10 mm ± 0,2 mm for 1/3-point flexure) and are free to roll inwards. The
2 © ISO 2012 – All rights reserved
rollers are free to rotate separately about an axis parallel to the length of the test piece to allow alignment.
For three-point flexure, the single loading roller, which need not rotate, shall be positioned centrally
between the outer-support rollers. The distances between the rollers shall be measured to the nearest
0,1 mm along the length of the specimen perpendicular to the direction of loading, using a travelling
microscope or other suitable device. The loading rollers in four-point flexure shall be symmetrically
positioned to within ± 0,1 mm. The arrangement for loading shall ensure that equal forces are applied
to the two loading rollers. The single loading roller in three-point flexure shall be centrally located to
within ± 0,2 mm.
5.6 Mechanical testing machine, capable of applying a force at a constant rate of displacement or
constant loading rate to the test piece in the flexural-strength test jig and of recording the force at which
the test piece fractures. The force measuring device shall be in accordance with ISO 7500-1 and shall have
an accuracy of ≤ 1 %.
NOTE The test facility can, with advantage, be equipped with a capability for recording the force/displacement
behaviour of the test piece, ideally a sensitive system directly contacting the test piece. Provided that the load-
train stiffness is sufficient, machine displacement recording can be adequate.
5.7 Ultrasonic cleaning bath, for cleaning the test pieces after notching, suitable for insertion of a
beaker or other receptacle containing solvent.
5.8 Calibrated micrometer, similar to the one in accordance with ISO 3611, but capable of being read
to a precision of 0,002 mm using a vernier or electronic readout.
5.9 Optical microscope, with calibrated magnifications over the range 50 × to 500 × , suitable for
observing the notch-tip shape, and fitted with photomicrographic facilities.
5.10 Notch-measuring device, a calibrated device for measuring the depth of the sawn notch after
fracture with a reading precision of 0,002 mm.
NOTE This can be achieved by the use of an appropriate travelling microscope, or a conventional metallurgical
microscope with calibrated stage movement, or a microscope with a calibrated micrometer eyepiece.
5.11 Drying oven, capable of maintaining 120 °C ± 5 °C for drying test pieces after cleaning.
5.12 Diamond slitting saw or slitting machine, capable of preparing a shallow notch in a set of test
pieces of width no more than 0,5 mm and depth of about 0,5 mm. See 6.3 for guidance.
6 Test piece preparation
6.1 Number of test pieces
At least seven test pieces shall be prepared for notching, of which five are required for testing and two
are dummy test pieces for protecting the others during notch preparation.
NOTE If a machine is used for preparing the V-notches, it might not be necessary to employ the dummy test
pieces to protect a test set of five test pieces.
Operators with no experience of preparing the sharp V-notches used in this method are highly
recommended to try out the technique and equipment first with surplus test pieces.
6.2 Test-piece dimensions
Prepare bar test pieces of rectangular cross-section, preferably in accordance with the requirements
of ISO 14704. Figure 1 shows the shape and main dimensions of the test pieces prepared in accordance
with this International Standard.
NOTE 1 The chamfering or rounding requirements in ISO 14704 are not essential for the V-notch test, and
can be ignored.
NOTE 2 Other sizes of test pieces, e.g. (2 × 2,5 × > 25 mm), can optionally be used with appropriately sized
flexural-strength fixtures.
Key
L > 45 mm (1/4-point flexure) or > 35 mm (1/3-point flexure)
W 4,0 mm ± 0,2 mm
B 3,0 mm ± 0,2 mm
Figure 1 — Test piece dimensions in accordance with ISO 14704
6.3 Preparing the V-notch by hand
Mount the test pieces side by side on the test-piece support using an appropriate temporary adhesive, as
in Figure 2. Mount test pieces and dummies as close together as possible. Ensure that the top surfaces
of the test pieces are level. Draw a pencil line across the set of test pieces at the mid-point of their length
to indicate where the notch is to be prepared. Bending the test pieces while mounting on the holder is
to be avoided.
4 © ISO 2012 – All rights reserved
Key
1 mounting plate
2 dummy test pieces
3 test pieces for testing
4 pencil line as a guide for introducing a diamond-sawn starter notch
Figure 2 — Mounting procedure for the set of test pieces
Mount the holder on a diamond saw. Saw a starter notch along the pencil line of width ≤ 0,5 mm. The
notch should have the same depth of about 0,5 mm over its entire length. Figure 3 shows a schematic
arrangement for sawing. After sawing, clean the holder, test pieces, and especially the notch.
Dimensions in millimetres
a) Test pieces arranged on the test piece support
b) Machining a starter notch with a thin diamond saw blade
Key
A tensile surface
B holder
C diamond saw blade
D sawn notch
X dummy test pieces
Figure 3 — Schematic diagrams for sawing
NOTE 1 It is helpful if the thickness of the diamond saw blade is only a little larger than the thickness of the
razor blade used for notch honing. Otherwise, the razor-blade tip might skate over the surface of the pre-sawn
notch and it might be difficult to start polishing the V-notch. V-shaping the saw-blade tip can help if available saw
blades are significantly thicker than the razor blades.
Fix the test-piece holder in a vice or other suitable clamp. Fill the starter notch with the fine diamond
paste as shown in Figure 4 a).
To protect the fingers, place a razor blade in a holder or apply a heavy self-adhesive tape as shown in
Figure 4 b). Put the exposed edge of the razor blade in the starter notch and apply a light force.
NOTE 2 Excessive force can be counter-productive, causing the razor-blade tip to blunt more quickly. Using a
force of about 5N to 10 N on the razor blade while polishing is normally sufficient.
Hone the V-notch with the razor blade with a smooth gentle back-and-forth motion [white arrows in
Figure 4 b)]. Move the razor blade as upright and level as possible.
NOTE 3 A drop of lubricating oil placed in the notch reduces any tendency for the razor blade to jerk or bind
while honing.
a) Applying diamond paste from a syringe to the sawn notch
b) Reciprocating a razor blade in the sawn notch
Key
1 heavy protection tape
2 razor blade
Figure 4 — Positioning a razor blade in the sawn notch
Examine the depth of the V-notch periodically with an optical microscope at both ends of the V-notch.
If possible, do not remove the test pieces from the test-piece holder for examination. If it is necessary to
remove them and further honing is required, remount the test pieces on the holder with a razor blade
inserted in the V-notch to act as a guide. If the total V-notch depth is less than 0,8 mm, continue to hone.
The total final V-notch depth should be between 0,8 mm and 1,2 mm.
NOTE 4 Honing by hand with a 4 µm diamond paste produces a V-notch width S of approximately 20 µm. Using
a finer diamond paste, e.g. a 1 µm one, usually does not decrease the width. If the V-notch width S is larger than
about 30 µm, it is suggested that a new razor blade or different razor-blade brand be employed. In coarse-grained
materials, large grains might pop out into the notch during honing and limit the ability to obtain a sharp V-notch.
6 © ISO 2012 – All rights reserved
NOTE 5 Different materials will take different periods of time to prepare the notch. Generally, harder or
tougher ceramics take longer than softer, more easily machined ceramics. Polishing V-notches into alumina test
pieces will take typically approximately 30 min and into silicon nitride ones typically approximately 4 h, for five
test pieces and two dummies.
Remove the test pieces from the holder while avoiding bending them. Carefully clean the test pieces with
acetone in a small powerful ultrasonic bath. Take care not to damage the test pieces while cleaning, e.g.
by allowing them to come into contact during ultrasonic cleaning. Dry the test pieces in the oven for at
least 1 h at 120 °C.
NOTE 6 Cleaning of the V-notch can be difficult, especially when the tip radius is small. Alternative steps might
be necessary to flush or scrape out the diamond grains.
6.4 Preparing the V-notches by machine (optional)
The task of honing V-notches can be automated. An example of a machine and its princ
...
INTERNATIONAL ISO
STANDARD 23146
Second edition
2012-12-15
Fine ceramics (advanced ceramics,
advanced technical ceramics) — Test
methods for fracture toughness of
monolithic ceramics — Single-edge
V-notch beam (SEVNB) method
Céramiques techniques — Méthodes d’essai pour la détermination de
la ténacité à la rupture des céramiques monolithiques — Méthode sur
éprouvette à entaille en V sur une seule face (Méthode SEVNB)
Reference number
©
ISO 2012
© ISO 2012
All rights reserved. Unless otherwise specified, no part of this publication may be reproduced or utilized in any form or by any
means, electronic or mechanical, including photocopying and microfilm, without permission in writing from either ISO at the
address below or ISO’s member body in the country of the requester.
ISO copyright office
Case postale 56 • CH-1211 Geneva 20
Tel. + 41 22 749 01 11
Fax + 41 22 749 09 47
E-mail copyright@iso.org
Web www.iso.org
Published in Switzerland
ii © ISO 2012 – All rights reserved
Contents Page
Foreword .iv
1 Scope . 1
2 Normative references . 1
3 Terms and definitions . 1
4 Principle . 1
5 Apparatus . 2
6 Test piece preparation . 3
6.1 Number of test pieces . 3
6.2 Test-piece dimensions . 4
6.3 Preparing the V-notch by hand . 4
6.4 Preparing the V-notches by machine (optional) . 7
6.5 Determination of notch-root radius . 7
7 Test procedure . 8
7.1 Dimensions of test piece . 8
7.2 Flexural-strength test . 8
7.3 Measurement of notch depth . 9
7.4 Calculation of fracture toughness . 9
8 Precision and bias .11
9 Test report .11
Annex A (informative) Notch honing by machine .12
Annex B (informative) Interlaboratory evaluation of the SEVNB fracture toughness
test procedures .14
Annex C (informative) Corrections for effective crack length greater than notch depth .16
Bibliography .17
Foreword
ISO (the International Organization for Standardization) is a worldwide federation of national standards
bodies (ISO member bodies). The work of preparing International Standards is normally carried out
through ISO technical committees. Each member body interested in a subject for which a technical
committee has been established has the right to be represented on that committee. International
organizations, governmental and non-governmental, in liaison with ISO, also take part in the work.
ISO collaborates closely with the International Electrotechnical Commission (IEC) on all matters of
electrotechnical standardization.
International Standards are drafted in accordance with the rules given in the ISO/IEC Directives, Part 2.
The main task of technical committees is to prepare International Standards. Draft International
Standards adopted by the technical committees are circulated to the member bodies for voting.
Publication as an International Standard requires approval by at least 75 % of the member bodies
casting a vote.
Attention is drawn to the possibility that some of the elements of this document may be the subject of
patent rights. ISO shall not be held responsible for identifying any or all such patent rights.
ISO 23146 was prepared by Technical Committee ISO/TC 206, Fine ceramics.
This second edition cancels and replaces the first edition (ISO 23146:2008), of which it constitutes a
minor revision.
iv © ISO 2012 – All rights reserved
INTERNATIONAL STANDARD ISO 23146:2012(E)
Fine ceramics (advanced ceramics, advanced technical
ceramics) — Test methods for fracture toughness of
monolithic ceramics — Single-edge V-notch beam
(SEVNB) method
1 Scope
This International Standard specifies a method for the determination of the fracture toughness of
advanced technical ceramics. The procedure makes use of single-edge V-notched bars, which are loaded
in four-point bending until failure. It is applicable to monolithic ceramics with a grain size or major
microstructural feature size larger than about 1 µm.
The use of this International Standard for yttria tetragonal zirconia polycrystal material (Y-TZP) is not
recommended. The method might also be unsuitable for some other very tough or soft ceramics in which
a sharp crack does not form at the root of the V-notch.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated
references, only the edition cited applies. For undated references, the latest edition of the referenced
document (including any amendments) applies.
ISO 3611, Geometrical product specifications (GPS) — Dimensional measuring instruments; Micrometers
for external measurements — Design and metrological characteristics
ISO 7500-1, Metallic materials — Verification of static uniaxial testing machines — Part 1: Tension/compression
testing machines — Verification and calibration of the force-measuring system
ISO 14704, Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for flexural
strength of monolithic ceramics at room temperature
ISO 15732, Fine ceramics (advanced ceramics, advanced technical ceramics) — Test method for fracture
toughness of monolithic ceramics at room temperature by single edge precracked beam (SEPB) method
3 Terms and definitions
For the purposes of this document, the terms and definitions given in ISO 15732 apply.
4 Principle
This method of conducting a fracture toughness test is based on the preparation and fracture of bar
test pieces in which a sharp-tipped notch is machined. Using the technique of a reciprocating razor
blade and diamond paste, a narrow notch can be honed into a test piece using either a manual method
or a simple machine. Under well-controlled conditions, a notch-tip radius in the range of 1 µm to 20 µm
can be prepared depending on the grain size of the test material. For many materials, this is a close
approximation to a sharp crack, and the method has been found to give fracture toughness values
very close to those of other methods such as the single-edge precracked beam method (ISO 15732) or
the surface crack in flexure method (ISO 18756), provided that a sharp crack forms at the root of the
notch either during its preparation or during the subsequent fracture sequence. The method has the
advantage of simplicity of notch production compared with using a sharp-tipped diamond saw or a
diamond impregnated wire in which the tip radius is normally greater than 50 µm. The method is often
easier to undertake compared with other methods of precracking and is applicable to a wider range of
materials outside the scope of these methods.
The method has been extensively researched (see the Bibliography) and has been evaluated in an ESIS
(European Structural Integrity Society)/VAMAS (Versailles Agreement on Advanced Materials and
Standards) round robin, the results of which are summarized in Annex B. This recommended practice is
based upon the ESIS/VAMAS SEVNB round robin.
The method may have some limitations for materials with grain sizes of less than 1 µm, for which
the assumption that the notch approximates to a sharp crack may not be valid (see Annex C). Users
should strive to minimize the notch-root radius in the test pieces. This International Standard places a
provisional criterion that the notch-root radius should be similar to or less than twice the average grain
size of the material.
The method is complementary to other methods of measuring fracture toughness described in ISO 15732
(single-edge precracked beam method), ISO 18756 (surface crack in flexure method), and ISO 24370
(chevron notch method); see the Bibliography.
5 Apparatus
5.1 Ordinary razor blades, preferably with a support along one edge but alternatively inserted in a
suitable holder.
NOTE 1 Razor blades thinner than about 0,2 mm are not ideal for this task unless stiffened by a support, such
as by gluing or screwing between two steel plates, leaving only about 2 mm of edge showing. A razor blade with a
tip angle of 30° or smaller is ideal.
NOTE 2 Although it is possible to machine the notches entirely by hand, the use of a simple device in which the
test pieces are mounted and in which a razor blade primed with diamond paste is moved in a reciprocating motion
across the mounted test pieces has a distinct advantage, as this provides controlled loading and directional
stability to the razor blade, and sharper notches are produced. An example is shown in Annex A.
5.2 Metallographic diamond paste, in a viscous organic carrier and of fine grain size, typically
1 µm to 3 µm.
5.3 Lubricant, a light lubricating oil for lubricating the razor blade, e.g. clock oil.
5.4 Test piece support, consisting of a flat plate or other suitable device for mounting test pieces
during notch honing.
5.5 Flexural-strength test fixture, preferably a four-point flexural-strength test fixture operating in
accordance with the requirements of ISO 14704, i.e. either 1/4-point flexure (preferred) or 1/3-point
flexure. Alternatively, a three-point flexural-strength test jig may also be used, but the alignment of the
V-notch with the central loading roller is more critical.
The test piece is supported on two bearing edges perpendicular to its length. The outer-support bearing
edges shall be parallel rollers of diameter 5,0 mm ± 0,2 mm and shall be capable of rolling outward on
flat support surfaces. Preferably, one of the rollers shall additionally be capable of rotating about an axis
parallel to the length of the test piece such that torsional loading is minimised. The two rollers shall
be positioned initially with their centres 40,0 mm ± 0,5 mm (1/4-point flexure) or 30 mm ± 0,5 mm
(1/3-point flexure) apart with their axes parallel to within 1°. The separation of the centres of the rollers
in their starting positions shall be measured to the nearest 0,1 mm with a travelling microscope. The
rollers shall be made from hardened steel or other hard material with a hardness greater than 40 HRC
(Rockwell C-scale). The rollers shall have a smooth burr-free surface finish with roughness less than
0,5 µm Ra and shall have a diameter uniform to ± 0,02 mm.
For four-point flexure, the two loading rollers are located at the 1/4-points (or 1/3-points), with an inner
span of 20 mm ± 0,2 mm (or 10 mm ± 0,2 mm for 1/3-point flexure) and are free to roll inwards. The
2 © ISO 2012 – All rights reserved
rollers are free to rotate separately about an axis parallel to the length of the test piece to allow alignment.
For three-point flexure, the single loading roller, which need not rotate, shall be positioned centrally
between the outer-support rollers. The distances between the rollers shall be measured to the nearest
0,1 mm along the length of the specimen perpendicular to the direction of loading, using a travelling
microscope or other suitable device. The loading rollers in four-point flexure shall be symmetrically
positioned to within ± 0,1 mm. The arrangement for loading shall ensure that equal forces are applied
to the two loading rollers. The single loading roller in three-point flexure shall be centrally located to
within ± 0,2 mm.
5.6 Mechanical testing machine, capable of applying a force at a constant rate of displacement or
constant loading rate to the test piece in the flexural-strength test jig and of recording the force at which
the test piece fractures. The force measuring device shall be in accordance with ISO 7500-1 and shall have
an accuracy of ≤ 1 %.
NOTE The test facility can, with advantage, be equipped with a capability for recording the force/displacement
behaviour of the test piece, ideally a sensitive system directly contacting the test piece. Provided that the load-
train stiffness is sufficient, machine displacement recording can be adequate.
5.7 Ultrasonic cleaning bath, for cleaning the test pieces after notching, suitable for insertion of a
beaker or other receptacle containing solvent.
5.8 Calibrated micrometer, similar to the one in accordance with ISO 3611, but capable of being read
to a precision of 0,002 mm using a vernier or electronic readout.
5.9 Optical microscope, with calibrated magnifications over the range 50 × to 500 × , suitable for
observing the notch-tip shape, and fitted with photomicrographic facilities.
5.10 Notch-measuring device, a calibrated device for measuring the depth of the sawn notch after
fracture with a reading precision of 0,002 mm.
NOTE This can be achieved by the use of an appropriate travelling microscope, or a conventional metallurgical
microscope with calibrated stage movement, or a microscope with a calibrated micrometer eyepiece.
5.11 Drying oven, capable of maintaining 120 °C ± 5 °C for drying test pieces after cleaning.
5.12 Diamond slitting saw or slitting machine, capable of preparing a shallow notch in a set of test
pieces of width no more than 0,5 mm and depth of about 0,5 mm. See 6.3 for guidance.
6 Test piece preparation
6.1 Number of test pieces
At least seven test pieces shall be prepared for notching, of which five are required for testing and two
are dummy test pieces for protecting the others during notch preparation.
NOTE If a machine is used for preparing the V-notches, it might not be necessary to employ the dummy test
pieces to protect a test set of five test pieces.
Operators with no experience of preparing the sharp V-notches used in this method are highly
recommended to try out the technique and equipment first with surplus test pieces.
6.2 Test-piece dimensions
Prepare bar test pieces of rectangular cross-section, preferably in accordance with the requirements
of ISO 14704. Figure 1 shows the shape and main dimensions of the test pieces prepared in accordance
with this International Standard.
NOTE 1 The chamfering or rounding requirements in ISO 14704 are not essential for the V-notch test, and
can be ignored.
NOTE 2 Other sizes of test pieces, e.g. (2 × 2,5 × > 25 mm), can optionally be used with appropriately sized
flexural-strength fixtures.
Key
L > 45 mm (1/4-point flexure) or > 35 mm (1/3-point flexure)
W 4,0 mm ± 0,2 mm
B 3,0 mm ± 0,2 mm
Figure 1 — Test piece dimensions in accordance with ISO 14704
6.3 Preparing the V-notch by hand
Mount the test pieces side by side on the test-piece support using an appropriate temporary adhesive, as
in Figure 2. Mount test pieces and dummies as close together as possible. Ensure that the top surfaces
of the test pieces are level. Draw a pencil line across the set of test pieces at the mid-point of their length
to indicate where the notch is to be prepared. Bending the test pieces while mounting on the holder is
to be avoided.
4 © ISO 2012 – All rights reserved
Key
1 mounting plate
2 dummy test pieces
3 test pieces for testing
4 pencil line as a guide for introducing a diamond-sawn starter notch
Figure 2 — Mounting procedure for the set of test pieces
Mount the holder on a diamond saw. Saw a starter notch along the pencil line of width ≤ 0,5 mm. The
notch should have the same depth of about 0,5 mm over its entire length. Figure 3 shows a schematic
arrangement for sawing. After sawing, clean the holder, test pieces, and especially the notch.
Dimensions in millimetres
a) Test pieces arranged on the test piece support
b) Machining a starter notch with a thin diamond saw blade
Key
A tensile surface
B holder
C diamond saw blade
D sawn notch
X dummy test pieces
Figure 3 — Schematic diagrams for sawing
NOTE 1 It is helpful if the thickness of the diamond saw blade is only a little larger than the thickness of the
razor blade used for notch honing. Otherwise, the razor-blade tip might skate over the surface of the pre-sawn
notch and it might be difficult to start polishing the V-notch. V-shaping the saw-blade tip can help if available saw
blades are significantly thicker than the razor blades.
Fix the test-piece holder in a vice or other suitable clamp. Fill the starter notch with the fine diamond
paste as shown in Figure 4 a).
To protect the fingers, place a razor blade in a holder or apply a heavy self-adhesive tape as shown in
Figure 4 b). Put the exposed edge of the razor blade in the starter notch and apply a light force.
NOTE 2 Excessive force can be counter-productive, causing the razor-blade tip to blunt more quickly. Using a
force of about 5N to 10 N on the razor blade while polishing is normally sufficient.
Hone the V-notch with the razor blade with a smooth gentle back-and-forth motion [white arrows in
Figure 4 b)]. Move the razor blade as upright and level as possible.
NOTE 3 A drop of lubricating oil placed in the notch reduces any tendency for the razor blade to jerk or bind
while honing.
a) Applying diamond paste from a syringe to the sawn notch
b) Reciprocating a razor blade in the sawn notch
Key
1 heavy protection tape
2 razor blade
Figure 4 — Positioning a razor blade in the sawn notch
Examine the depth of the V-notch periodically with an optical microscope at both ends of the V-notch.
If possible, do not remove the test pieces from the test-piece holder for examination. If it is necessary to
remove them and further honing is required, remount the test pieces on the holder with a razor blade
inserted in the V-notch to act as a guide. If the total V-notch depth is less than 0,8 mm, continue to hone.
The total final V-notch depth should be between 0,8 mm and 1,2 mm.
NOTE 4 Honing by hand with a 4 µm diamond paste produces a V-notch width S of approximately 20 µm. Using
a finer diamond paste, e.g. a 1 µm one, usually does not decrease the width. If the V-notch width S is larger than
about 30 µm, it is suggested that a new razor blade or different razor-blade brand be employed. In coarse-grained
materials, large grains might pop out into the notch during honing and limit the ability to obtain a sharp V-notch.
6 © ISO 2012 – All rights reserved
NOTE 5 Different materials will take different periods of time to prepare the notch. Generally, harder or
tougher ceramics take longer than softer, more easily machined ceramics. Polishing V-notches into alumina test
pieces will take typically approximately 30 min and into silicon nitride ones typically approximately 4 h, for five
test pieces and two dummies.
Remove the test pieces from the holder while avoiding bending them. Carefully clean the test pieces with
acetone in a small powerful ultrasonic bath. Take care not to damage the test pieces while cleaning, e.g.
by allowing them to come into contact during ultrasonic cleaning. Dry the test pieces in the oven for at
least 1 h at 120 °C.
NOTE 6 Cleaning of the V-notch can be difficult, especially when the tip radius is small. Alternative steps might
be necessary to flush or scrape out the diamond grains.
6.4 Preparing the V-notches by machine (optional)
The task of honing V-notches can be automated. An example of a machine and its princ
...
NORME ISO
INTERNATIONALE 23146
Deuxième édition
2012-12-15
Céramiques techniques — Méthodes
d’essai pour la détermination de la
ténacité à la rupture des céramiques
monolithiques — Méthode sur
éprouvette à entaille en V sur une
seule face (Méthode SEVNB)
Fine ceramics (advanced ceramics, advanced technical ceramics) —
Test methods for fracture toughness of monolithic ceramics — Single-
edge V-notch beam (SEVNB) method
Numéro de référence
©
ISO 2012
DOCUMENT PROTÉGÉ PAR COPYRIGHT
© ISO 2012
Droits de reproduction réservés. Sauf indication contraire, aucune partie de cette publication ne peut être reproduite ni utilisée
sous quelque forme que ce soit et par aucun procédé, électronique ou mécanique, y compris la photocopie, l’affichage sur
l’internet ou sur un Intranet, sans autorisation écrite préalable. Les demandes d’autorisation peuvent être adressées à l’ISO à
l’adresse ci-après ou au comité membre de l’ISO dans le pays du demandeur.
ISO copyright office
Case postale 56 • CH-1211 Geneva 20
Tel. + 41 22 749 01 11
Fax + 41 22 749 09 47
E-mail copyright@iso.org
Web www.iso.org
Version française parue en 2013
Publié en Suisse
ii © ISO 2012 – Tous droits réservés
Sommaire Page
Avant-propos .iv
1 Domaine d’application . 1
2 Références normatives . 1
3 Termes et définitions . 1
4 Principe . 1
5 Appareillage . 2
6 Préparation des éprouvettes . 4
6.1 Nombre d’éprouvettes . 4
6.2 Dimensions des éprouvettes . 4
6.3 Préparation manuelle de l’entaille en V . 4
6.4 Préparation des entailles en V à la machine (en option) . 8
6.5 Détermination du rayon à fond d’entaille . 8
7 Méthode d’essai . 9
7.1 Dimensions de l’éprouvette . 9
7.2 Essai de résistance en flexion . 9
7.3 Mesure de la profondeur de l’entaille .10
7.4 Calcul de la ténacité à la rupture .11
8 Fidélité et biais .12
9 Rapport d’essai .13
Annexe A (informative) Affûtage des entailles à la machine .14
Annexe B (informative) Évaluation interlaboratoires des méthodes SEVNB d’essai de ténacité à
la rupture .16
Annexe C (informative) Corrections relatives à la longueur réelle de la fissure plus élevée que la
profondeur de l’entaille .18
Bibliographie .20
Avant-propos
L’ISO (Organisation internationale de normalisation) est une fédération mondiale d’organismes
nationaux de normalisation (comités membres de l’ISO). L’élaboration des Normes internationales est
en général confiée aux comités techniques de l’ISO. Chaque comité membre intéressé par une étude
a le droit de faire partie du comité technique créé à cet effet. Les organisations internationales,
gouvernementales et non gouvernementales, en liaison avec l’ISO participent également aux travaux.
L’ISO collabore étroitement avec la Commission électrotechnique internationale (CEI) en ce qui concerne
la normalisation électrotechnique.
Les Normes internationales sont rédigées conformément aux règles données dans les Directives
ISO/CEI, Partie 2.
La tâche principale des comités techniques est d’élaborer les Normes internationales. Les projets de
Normes internationales adoptés par les comités techniques sont soumis aux comités membres pour vote.
Leur publication comme Normes internationales requiert l’approbation de 75 % au moins des comités
membres votants.
L’attention est appelée sur le fait que certains des éléments du présent document peuvent faire l’objet de
droits de propriété intellectuelle ou de droits analogues. L’ISO ne saurait être tenue pour responsable de
ne pas avoir identifié de tels droits de propriété et averti de leur existence.
L’ISO 23146 a été élaborée par le comité technique ISO/TC 206, Céramiques techniques.
Cette deuxième édition annule et remplace la première édition (ISO 23146:2008) qui a fait l’objet d’une
révision mineure.
iv © ISO 2012 – Tous droits réservés
NORME INTERNATIONALE ISO 23146:2012(F)
Céramiques techniques — Méthodes d’essai pour la
détermination de la ténacité à la rupture des céramiques
monolithiques — Méthode sur éprouvette à entaille en V
sur une seule face (Méthode SEVNB)
1 Domaine d’application
La présente Norme internationale spécifie une méthode d’essai pour la détermination de la ténacité à
la rupture des céramiques techniques. La méthode utilise des éprouvettes à entaille en V sur une seule
face, qui sont chargées en flexion quatre points jusqu’à la rupture. Elle est applicable aux céramiques
monolithiques avec une taille de grains ou une taille des principales caractéristiques microstructurales
supérieure à environ 1 µm.
Il n’est pas recommandé d’utiliser la présente Norme internationale pour le matériau polycristallin de
zircone tétragonale d’yttria (Y-TZP). La méthode peut aussi ne pas convenir à d’autres céramiques très
tenaces ou molles dans lesquelles une fissure tranchante ne se forme pas à la racine de l’entaille en V.
2 Références normatives
Les documents suivants, en tout ou partie, sont référencés de manière normative dans le présent
document et sont indispensables pour son application. Pour les références datées, seule l’édition citée
s’applique. Pour les références non datées, la dernière édition du document de référence s’applique (y
compris les éventuels amendements).
ISO 3611, Spécification géométrique des produits (GPS) — Équipement de mesurage dimensionnel:
Micromètres d’extérieur — Caractéristiques de conception et caractéristiques métrologiques
ISO 7500-1, Matériaux métalliques — Vérification des machines pour essais statiques uniaxiaux — Partie 1:
Machines d’essai de traction/compression — Vérification et étalonnage du système de mesure de force
ISO 14704, Céramiques techniques — Méthode d’essai de résistance en flexion des céramiques monolithiques
à température ambiante
ISO 15732, Céramiques techniques — Méthode d’essai de ténacité à la rupture des céramiques monolithiques
à température ambiante sur éprouvette préfissurée sur une seule face (méthode SEPB)
3 Termes et définitions
Pour les besoins du présent document, les termes et définitions donnés dans l’ISO 15732 s’appliquent.
4 Principe
La présente méthode d’essai de ténacité à la rupture est basée sur la préparation et la rupture
d’éprouvettes en barres dans lesquelles une entaille à extrémité tranchante est usinée. L’application de
la technique de la lame de rasoir à mouvement alternatif et de la pâte de diamant permet d’affûter une
petite entaille dans une éprouvette à l’aide d’une méthode manuelle ou d’une machine simple. Dans des
conditions bien contrôlées, une extrémité d’entaille dont le rayon se situe dans la plage de 1 µm à 20 µm
peut être préparée sur la base de la taille des grains du matériau d’essai. Pour bon nombre de matériaux,
il s’agit d’une approximation proche d’une fissure tranchante; cette méthode s’est par ailleurs révélée
donner des valeurs de ténacité à la rupture très proches de celles d’autres méthodes telles que la méthode
de l’éprouvette préfissurée sur une seule face (ISO 15732) ou la méthode par fissuration superficielle en
flexion (ISO 18756) à condition qu’une fissure tranchante se forme à la racine de l’entaille soit pendant la
préparation soit pendant la séquence de rupture qui suit. La méthode présente l’avantage de simplifier
la production des entailles par rapport à l’utilisation d’une scie diamantée à extrémité tranchante ou
d’un câble imprégné de diamant pour lequel le rayon de l’extrémité est normalement supérieur à 50 µm.
La méthode est souvent plus facile à utiliser que d’autres méthodes de préfissuration et s’applique à une
gamme plus étendue de matériaux ne relevant pas du domaine d’application de ces méthodes.
La méthode a fait l’objet de recherches approfondies (voir la Bibliographie) et a été évaluée au titre d’une
étude comparative interlaboratoires de ESIS (European Structural Integrity Society)/VAMAS (Versailles
Agreement on Advanced Materials and Standards), dont les résultats sont résumés à l’Annexe B. Cette
pratique recommandée est basée sur l’essai comparatif interlaboratoires de SEVNB par ESIS/VAMAS.
La méthode peut comporter certaines limites applicables aux matériaux dont les grains ont une taille de
moins de 1 µm, pour laquelle l’hypothèse selon laquelle l’entaille a une valeur proche de la valeur d’une
fissure tranchante peut ne pas être valide (voir Annexe C). Il convient que les utilisateurs s’efforcent de
réduire le rayon à fond d’entaille dans les éprouvettes d’essai. La présente Norme internationale établit
un critère provisoire suivant lequel il convient que le rayon à fond d’entaille soit similaire ou inférieur
au double de la taille moyenne des grains du matériau.
La méthode est complémentaire aux autres méthodes de mesure de la ténacité à la rupture décrites
dans l’ISO 15732 (méthode de l’éprouvette préfissurée sur une seule face), l’ISO 18756 (méthode par
fissuration superficielle en flexion) et l’ISO 24370 (méthode de l’entaille en chevron); voir la Bibliographie.
5 Appareillage
5.1 Lames de rasoir ordinaires, de préférence avec un support le long d’une face mais insérées en
option dans un porte-lames adéquat.
NOTE 1 Des lames de rasoir plus minces que 0,2 mm environ ne conviennent pas bien à cette tâche, à moins
qu’elles soient renforcées par un support; par exemple en les collant ou en les vissant entre deux plaques d’acier,
pour ne laisser apparaître qu’une face d’environ 2 mm. Une lame de rasoir avec un angle de tête de 30° ou plus
petit est l’idéal.
NOTE 2 Bien qu’il soit possible de réaliser les entailles entièrement à la main, l’utilisation d’un dispositif simple
dans lequel les éprouvettes sont montées et dans lequel une lame de rasoir couverte d’une pâte de diamant est
déplacée dans un mouvement alternatif à travers les éprouvettes montées présente l’avantage de pouvoir contrôler
la charge, assurer une stabilité directionnelle à la lame de rasoir et produire des entailles plus tranchantes. Un
exemple de ce dispositif est présenté dans l’Annexe A.
5.2 Pâte de diamant métallographique, dans un porteur organique visqueux et ayant une taille de
grains fins, généralement entre 1 µm et 3 µm.
5.3 Lubrifiant, une huile lubrifiante légère pour lubrifier la lame de rasoir, par exemple huile pour horloge.
5.4 Support d’éprouvettes, comprenant une plaque plane ou autre dispositif approprié destiné au
montage des éprouvettes pendant l’affûtage des entailles.
5.5 Dispositif d’essai de résistance en flexion, de préférence, un dispositif d’essai de résistance
en flexion quatre points fonctionnant conformément aux exigences de l’ISO 14704, c’est-à-dire soit en
flexion 1/4 de point (préférée) soit en flexion 1/3 de point. En variante, un montage d’essai de résistance
en flexion trois points peut aussi être utilisé, mais l’alignement de l’entaille en V avec le cylindre de charge
central est plus critique.
L’éprouvette est supportée par deux rebords portants perpendiculaires à sa longueur. Les rebords
portants externes du support doivent être des cylindres parallèles de 5,0 mm ± 0,2 mm de diamètre
et doivent être capables de rouler à l’extérieur sur des surfaces d’appui planes. De préférence, un des
cylindres doit de plus être capable de tourner autour d’un axe parallèle à la longueur de l’éprouvette de
sorte que la charge de torsion soit réduite. Les deux cylindres doivent être au départ positionnés avec
leurs centres distants de 40,0 mm ± 0,5 mm (flexion 1/4 de point) ou 30 mm ± 0,5 mm (flexion 1/3 de
2 © ISO 2012 – Tous droits réservés
point) et leurs axes parallèles à 1° environ. La séparation des centres des cylindres dans leurs positions
initiales doit être mesurée à 0,1 mm près avec un microscope mobile. Les cylindres doivent être en acier
trempé ou autre matériau dur de dureté supérieure à 40 HRC (échelle de Rockwell C). Les cylindres
doivent avoir un fini de surface lisse sans bavures avec une ténacité inférieure à 0,5 µm Ra, et avoir un
diamètre uniforme égal à ± 0,02 mm.
Pour la flexion quatre points, les deux cylindres de charge sont placés à 1/4 de point (ou 1/3 de point), avec
une portée interne de 20 mm ± 0,2 mm (ou 10 mm ± 0,2 mm pour la flexion 1/3 de point) et sont libres de
rouler à l’intérieur. Les cylindres sont libres de pivoter séparément autour d’un axe parallèle à la longueur
de l’éprouvette pour permettre l’alignement. Pour la flexion trois points, le cylindre de charge unique,
qui n’a pas besoin de pivoter, doit être positionné au centre entre les cylindres d’appui externes. Les
distances entre les cylindres doivent être mesurées à 0,1 mm près le long de la longueur de l’éprouvette
perpendiculaire à la direction de charge, à l’aide d’un microscope mobile ou autre dispositif adéquat. Les
cylindres de charge en flexion quatre points doivent être positionnés de façon symétrique à ± 0,1 mm
environ. Le dispositif de charge doit assurer que des forces identiques sont appliquées aux deux cylindres
de charge. Le cylindre de charge unique en flexion trois points doit être placé au centre à ± 0,2 mm.
5.6 Machine d’essai mécanique, capable d’appliquer une force à une vitesse constante de déplacement
ou de charge sur l’éprouvette dans le montage d’essai de résistance en flexion, et d’enregistrer la force
à laquelle la rupture de l’éprouvette survient. Le dispositif de mesure de la force doit être en conformité
avec l’ISO 7500-1 et doit avoir une exactitude ≤ 1 %.
NOTE L’équipement d’essai peut également bénéficier d’une capacité d’enregistrement de la force/du
comportement de déplacement de l’éprouvette; théoriquement il peut s’agir d’un système sensible directement
en contact avec l’éprouvette. Sous réserve d’une rigidité suffisante du train de charges, l’enregistrement du
déplacement de la machine peut être satisfaisant.
5.7 Bain de nettoyage par ultrasons, pour nettoyer les éprouvettes après entaillage, approprié pour
l’insertion d’un bécher ou autre récipient contenant du solvant.
5.8 Micromètre étalonné, similaire à celui décrit dans l’ISO 3611, mais capable d’être lu à une
résolution de 0,002 mm à l’aide d’un vernier ou d’une unité de lecture électronique.
5.9 Microscope optique, avec des grossissements étalonnés sur la plage × 50 à × 500, approprié pour
observer la forme de l’extrémité de l’entaille et muni d’équipements photo-micrographiques.
5.10 Dispositif de mesure de l’entaille, dispositif étalonné pour mesurer la profondeur de l’entaille
sciée après rupture avec une précision de lecture de 0,002 mm.
NOTE Cette profondeur peut être mesurée à l’aide d’un microscope mobile approprié ou d’un microscope
métallurgique conventionnel avec mouvement par étapes étalonné, ou d’un oculaire de réglage à micromètre étalonné.
5.11 Four de séchage, capable de maintenir une température de 120 °C ± 5 °C pour sécher les éprouvettes
après nettoyage.
5.12 Scie diamantée à refendre ou machine à refendre, capable de préparer une entaille peu profonde
dans un ensemble d’éprouvettes de 0,5 mm de large au maximum et d’une profondeur d’environ 0,5 mm.
Voir 6.3 pour des lignes directrices.
6 Préparation des éprouvettes
6.1 Nombre d’éprouvettes
Au moins sept éprouvettes doivent être préparées pour l’entaillage, dont cinq sont nécessaires pour
les essais et deux sont des éprouvettes factices destinées à la protection des cinq autres pendant la
préparation des entailles.
NOTE Si une machine est utilisée pour préparer les entailles en V, il peut ne pas être nécessaire d’utiliser les
éprouvettes factices pour protéger un banc d’essai de cinq éprouvettes.
Il est fortement recommandé aux opérateurs sans aucune expérience dans la préparation des entailles
tranchantes en V utilisées pour cette méthode de s’entraîner tout d’abord à la technique et aux matériels
avec des éprouvettes supplémentaires.
6.2 Dimensions des éprouvettes
Préparer des éprouvettes d’essai en barre de section rectangulaire, de préférence en conformité avec
les exigences de l’ISO 14704. La Figure 1 présente la forme et les dimensions principales des éprouvettes
préparées conformément à la présente Norme internationale.
NOTE 1 Les exigences de chanfreinage ou d’arrondi spécifiées dans l’ISO 14704 ne sont pas indispensables
pour l’essai des entailles en V et peuvent donc être ignorées.
NOTE 2 D’autres dimensions d’éprouvettes, par exemple (2 × 2,5 × > 25 mm) peuvent en option être utilisées
avec des dispositifs de résistance en flexion dimensionnés de manière appropriée.
Légende
L (longueur) > 45 mm (flexion 1/4 de point) ou > 35 mm (flexion 1/3 de point)
W (profondeur) 4,0 mm ± 0,2 mm
B (largeur) 3,0 mm ± 0,2 mm
Figure 1 — Dimensions de l’éprouvette conformément à l’ISO 14704
6.3 Préparation manuelle de l’entaille en V
Monter les éprouvettes côte à côte sur le support d’éprouvettes à l’aide d’un adhésif temporaire approprié,
tel qu’il est indiqué à la Figure 2. Monter les éprouvettes d’essai et les éprouvettes factices aussi proches
que possible. Veiller à ce que les faces supérieures des éprouvettes soient mises à niveau. Tracer au
4 © ISO 2012 – Tous droits réservés
crayon une ligne sur l’ensemble des éprouvettes au milieu de leur longueur, pour indiquer l’endroit où
l’entaille est à préparer. Le fléchissement des éprouvettes lors de leur montage sur le support est à éviter.
Légende
1 plaque de montage
2 éprouvettes factices
3 éprouvettes d’essai
4 ligne au crayon comme guide d’insertion d’une entaille d’amorce faite par une scie diamantée
Figure 2 — Procédure de montage de l’ensemble des éprouvettes
Monter le support sur une scie diamantée. Scier une entaille d’amorce le long du trait au crayon de
largeur ≤ 0,5 mm. Il convient que l’entaille ait la même profondeur de 0,5 mm environ sur toute sa
longueur. La Figure 3 présente un schéma du sciage. Après le sciage, nettoyer le support, les éprouvettes
et plus particulièrement l’entaille.
Dimensions en millimètres
a) Éprouvettes disposées sur le support d’éprouvettes
b) Usinage d’une entaille d’amorce avec une scie à lame diamantée mince
Légende
A surface de traction
B support
C lame de scie diamantée
D entaille sciée
X éprouvettes factices
Figure 3 — Schémas de sciage
NOTE 1 Il est utile que l’épaisseur de la lame de scie diamantée soit juste un peu plus grande que l’épaisseur
de la lame de rasoir utilisée pour l’affûtage de l’entaille. Sinon, l’extrémité de la lame de rasoir pourrait recouvrir
la surface de l’entaille pré-sciée et il pourrait être difficile de commencer le polissage de l’entaille en V. L’usinage
en V de l’extrémité de la lame de scie peut être utile lorsque les lames de scie disponibles sont sensiblement plus
épaisses que les lames de rasoir.
Fixer le support d’éprouvettes dans un étau ou autre dispositif de blocage approprié. Remplir l’entaille
d’amorce de la pâte de diamant fine, tel qu’il est présenté à la Figure 4 a).
Pour protéger les doigts, placer une lame de rasoir dans un porte-lames ou appliquer une bande
autoadhésive épaisse, tel qu’il est présenté à la Figure 4 b). Mettre la face exposée de la lame de rasoir
dans l’entaille d’amorce et exercer une force légère.
NOTE 2 Une force excessive peut être contre-productive, causant l’émoussement plus rapide de l’extrémité de
la lame de rasoir. L’application d’une force d’environ 5 N à 10 N sur la lame de rasoir pendant le polissage est
normalement suffisante.
Affûter l’entaille en V avec la lame de rasoir avec un mouvement de va et vient souple et doux [flèches
blanches à la Figure 4 b)]. Déplacer la lame de rasoir de façon aussi verticale et horizontale que possible.
NOTE 3 Une goutte d’huile lubrifiante versée sur l’entaille réduit toute saccade éventuelle ou tout coincement
éventuel de la lame de rasoir pendant l’affûtage.
6 © ISO 2012 – Tous droits réservés
a) Application de la pâte de diamant à l’aide d’une seringue sur l’entaille sciée
b) Lame de rasoir en mouvement alternatif dans l’entaille sciée
Légende
1 bande de protection épaisse
2 lame de rasoir
Figure 4 — Positionnement d’une lame de rasoir dans l’entaille sciée
Examiner périodiquement la profondeur de l’entaille en V à l’aide d’un microscope optique aux deux
extrémités de l’entaille en V. Dans toute la mesure du possible, examiner les éprouvettes sans les retirer
du porte-éprouvettes. S’il est nécessaire de les retirer et si un affûtage complémentaire est requis,
monter à nouveau les éprouvettes sur le support en insérant une lame de rasoir dans l’entaille en V pour
servir de guide. Si la profondeur totale de l’entaille en V est inférieure à 0,8 mm, poursuivre l’affûtage. Il
convient que la profondeur totale de l’entaille en V soit comprise entre 0,8 mm et 12 mm.
NOTE 4 L’affûtage manuel à l’aide d’une pâte de diamant de 4 µm produit une entaille en V de largeur S
d’environ 20 µm. L’utilisation d’une pâte de diamant plus fine, par exemple de 1 µm, ne diminue généralement pas
la largeur. Si la largeur S de l’entaille en V est supérieure à 30 µm environ, il est recommandé d’utiliser une nouvelle
lame de rasoir ou une marque différente de lame de rasoir. Pour les matériaux à gros grains, les gros grains
peuvent sauter dans l’entaille lors de l’affûtage et limiter ainsi la capacité à obtenir une entaille en V tranchante.
NOTE 5 Des matériaux différents nécessitent des périodes de temps différentes pour la préparation de l’entaille.
En général, les céramiques plus dures ou plus tenaces prennent plus de temps que les céramiques plus souples,
plus facilement usinées. Le polissage des entailles en V dans des éprouvettes d’alumine prend généralement
environ 30 min, et dans des éprouvettes de nitrure de silicium environ 4 h, pour cinq éprouvettes d’essai et deux
éprouvettes factices.
Retirer les éprouvettes du support tout en évitant de les plier. Nettoyer soigneusement les éprouvettes
avec de l’acétone dans un petit bain à ultrasons puissants. Veiller à ne pas endommager les éprouvettes
pendant le nettoyage, par exemple en leur permettant d’être en contact pendant le nettoyage par
ultrasons. Sécher les éprouvettes dans l’étuve pendant au moins 1 h à 120 °C.
NOTE 6 Le nettoyage de l’entaille en V peut être difficile, notamment lorsque le rayon de l’extrémité est petit.
Des mesures alternatives peuvent s’avérer nécessaires pour épurer ou gratter les grains de diamant.
6.4 Préparation des entailles en V à la machine (en option)
L’opération d’affûtage des entailles en V peut être automatisée. L’Annexe A présente à cet effet un exemple
de machine et les exigences principales qui s’y appliquent.
NOTE 1 Avec une machine de rigidité suffisante utilisant une pâte de diamant de 1 µm pour les phases finales
d’entaillage, la largeur de l’entaille peu
...
NORME ISO
INTERNATIONALE 23146
Deuxième édition
2012-12-15
Céramiques techniques — Méthodes
d’essai pour la détermination de la
ténacité à la rupture des céramiques
monolithiques — Méthode sur
éprouvette à entaille en V sur une
seule face (Méthode SEVNB)
Fine ceramics (advanced ceramics, advanced technical ceramics) —
Test methods for fracture toughness of monolithic ceramics — Single-
edge V-notch beam (SEVNB) method
Numéro de référence
©
ISO 2012
DOCUMENT PROTÉGÉ PAR COPYRIGHT
© ISO 2012
Droits de reproduction réservés. Sauf indication contraire, aucune partie de cette publication ne peut être reproduite ni utilisée
sous quelque forme que ce soit et par aucun procédé, électronique ou mécanique, y compris la photocopie, l’affichage sur
l’internet ou sur un Intranet, sans autorisation écrite préalable. Les demandes d’autorisation peuvent être adressées à l’ISO à
l’adresse ci-après ou au comité membre de l’ISO dans le pays du demandeur.
ISO copyright office
Case postale 56 • CH-1211 Geneva 20
Tel. + 41 22 749 01 11
Fax + 41 22 749 09 47
E-mail copyright@iso.org
Web www.iso.org
Version française parue en 2013
Publié en Suisse
ii © ISO 2012 – Tous droits réservés
Sommaire Page
Avant-propos .iv
1 Domaine d’application . 1
2 Références normatives . 1
3 Termes et définitions . 1
4 Principe . 1
5 Appareillage . 2
6 Préparation des éprouvettes . 4
6.1 Nombre d’éprouvettes . 4
6.2 Dimensions des éprouvettes . 4
6.3 Préparation manuelle de l’entaille en V . 4
6.4 Préparation des entailles en V à la machine (en option) . 8
6.5 Détermination du rayon à fond d’entaille . 8
7 Méthode d’essai . 9
7.1 Dimensions de l’éprouvette . 9
7.2 Essai de résistance en flexion . 9
7.3 Mesure de la profondeur de l’entaille .10
7.4 Calcul de la ténacité à la rupture .11
8 Fidélité et biais .12
9 Rapport d’essai .13
Annexe A (informative) Affûtage des entailles à la machine .14
Annexe B (informative) Évaluation interlaboratoires des méthodes SEVNB d’essai de ténacité à
la rupture .16
Annexe C (informative) Corrections relatives à la longueur réelle de la fissure plus élevée que la
profondeur de l’entaille .18
Bibliographie .20
Avant-propos
L’ISO (Organisation internationale de normalisation) est une fédération mondiale d’organismes
nationaux de normalisation (comités membres de l’ISO). L’élaboration des Normes internationales est
en général confiée aux comités techniques de l’ISO. Chaque comité membre intéressé par une étude
a le droit de faire partie du comité technique créé à cet effet. Les organisations internationales,
gouvernementales et non gouvernementales, en liaison avec l’ISO participent également aux travaux.
L’ISO collabore étroitement avec la Commission électrotechnique internationale (CEI) en ce qui concerne
la normalisation électrotechnique.
Les Normes internationales sont rédigées conformément aux règles données dans les Directives
ISO/CEI, Partie 2.
La tâche principale des comités techniques est d’élaborer les Normes internationales. Les projets de
Normes internationales adoptés par les comités techniques sont soumis aux comités membres pour vote.
Leur publication comme Normes internationales requiert l’approbation de 75 % au moins des comités
membres votants.
L’attention est appelée sur le fait que certains des éléments du présent document peuvent faire l’objet de
droits de propriété intellectuelle ou de droits analogues. L’ISO ne saurait être tenue pour responsable de
ne pas avoir identifié de tels droits de propriété et averti de leur existence.
L’ISO 23146 a été élaborée par le comité technique ISO/TC 206, Céramiques techniques.
Cette deuxième édition annule et remplace la première édition (ISO 23146:2008) qui a fait l’objet d’une
révision mineure.
iv © ISO 2012 – Tous droits réservés
NORME INTERNATIONALE ISO 23146:2012(F)
Céramiques techniques — Méthodes d’essai pour la
détermination de la ténacité à la rupture des céramiques
monolithiques — Méthode sur éprouvette à entaille en V
sur une seule face (Méthode SEVNB)
1 Domaine d’application
La présente Norme internationale spécifie une méthode d’essai pour la détermination de la ténacité à
la rupture des céramiques techniques. La méthode utilise des éprouvettes à entaille en V sur une seule
face, qui sont chargées en flexion quatre points jusqu’à la rupture. Elle est applicable aux céramiques
monolithiques avec une taille de grains ou une taille des principales caractéristiques microstructurales
supérieure à environ 1 µm.
Il n’est pas recommandé d’utiliser la présente Norme internationale pour le matériau polycristallin de
zircone tétragonale d’yttria (Y-TZP). La méthode peut aussi ne pas convenir à d’autres céramiques très
tenaces ou molles dans lesquelles une fissure tranchante ne se forme pas à la racine de l’entaille en V.
2 Références normatives
Les documents suivants, en tout ou partie, sont référencés de manière normative dans le présent
document et sont indispensables pour son application. Pour les références datées, seule l’édition citée
s’applique. Pour les références non datées, la dernière édition du document de référence s’applique (y
compris les éventuels amendements).
ISO 3611, Spécification géométrique des produits (GPS) — Équipement de mesurage dimensionnel:
Micromètres d’extérieur — Caractéristiques de conception et caractéristiques métrologiques
ISO 7500-1, Matériaux métalliques — Vérification des machines pour essais statiques uniaxiaux — Partie 1:
Machines d’essai de traction/compression — Vérification et étalonnage du système de mesure de force
ISO 14704, Céramiques techniques — Méthode d’essai de résistance en flexion des céramiques monolithiques
à température ambiante
ISO 15732, Céramiques techniques — Méthode d’essai de ténacité à la rupture des céramiques monolithiques
à température ambiante sur éprouvette préfissurée sur une seule face (méthode SEPB)
3 Termes et définitions
Pour les besoins du présent document, les termes et définitions donnés dans l’ISO 15732 s’appliquent.
4 Principe
La présente méthode d’essai de ténacité à la rupture est basée sur la préparation et la rupture
d’éprouvettes en barres dans lesquelles une entaille à extrémité tranchante est usinée. L’application de
la technique de la lame de rasoir à mouvement alternatif et de la pâte de diamant permet d’affûter une
petite entaille dans une éprouvette à l’aide d’une méthode manuelle ou d’une machine simple. Dans des
conditions bien contrôlées, une extrémité d’entaille dont le rayon se situe dans la plage de 1 µm à 20 µm
peut être préparée sur la base de la taille des grains du matériau d’essai. Pour bon nombre de matériaux,
il s’agit d’une approximation proche d’une fissure tranchante; cette méthode s’est par ailleurs révélée
donner des valeurs de ténacité à la rupture très proches de celles d’autres méthodes telles que la méthode
de l’éprouvette préfissurée sur une seule face (ISO 15732) ou la méthode par fissuration superficielle en
flexion (ISO 18756) à condition qu’une fissure tranchante se forme à la racine de l’entaille soit pendant la
préparation soit pendant la séquence de rupture qui suit. La méthode présente l’avantage de simplifier
la production des entailles par rapport à l’utilisation d’une scie diamantée à extrémité tranchante ou
d’un câble imprégné de diamant pour lequel le rayon de l’extrémité est normalement supérieur à 50 µm.
La méthode est souvent plus facile à utiliser que d’autres méthodes de préfissuration et s’applique à une
gamme plus étendue de matériaux ne relevant pas du domaine d’application de ces méthodes.
La méthode a fait l’objet de recherches approfondies (voir la Bibliographie) et a été évaluée au titre d’une
étude comparative interlaboratoires de ESIS (European Structural Integrity Society)/VAMAS (Versailles
Agreement on Advanced Materials and Standards), dont les résultats sont résumés à l’Annexe B. Cette
pratique recommandée est basée sur l’essai comparatif interlaboratoires de SEVNB par ESIS/VAMAS.
La méthode peut comporter certaines limites applicables aux matériaux dont les grains ont une taille de
moins de 1 µm, pour laquelle l’hypothèse selon laquelle l’entaille a une valeur proche de la valeur d’une
fissure tranchante peut ne pas être valide (voir Annexe C). Il convient que les utilisateurs s’efforcent de
réduire le rayon à fond d’entaille dans les éprouvettes d’essai. La présente Norme internationale établit
un critère provisoire suivant lequel il convient que le rayon à fond d’entaille soit similaire ou inférieur
au double de la taille moyenne des grains du matériau.
La méthode est complémentaire aux autres méthodes de mesure de la ténacité à la rupture décrites
dans l’ISO 15732 (méthode de l’éprouvette préfissurée sur une seule face), l’ISO 18756 (méthode par
fissuration superficielle en flexion) et l’ISO 24370 (méthode de l’entaille en chevron); voir la Bibliographie.
5 Appareillage
5.1 Lames de rasoir ordinaires, de préférence avec un support le long d’une face mais insérées en
option dans un porte-lames adéquat.
NOTE 1 Des lames de rasoir plus minces que 0,2 mm environ ne conviennent pas bien à cette tâche, à moins
qu’elles soient renforcées par un support; par exemple en les collant ou en les vissant entre deux plaques d’acier,
pour ne laisser apparaître qu’une face d’environ 2 mm. Une lame de rasoir avec un angle de tête de 30° ou plus
petit est l’idéal.
NOTE 2 Bien qu’il soit possible de réaliser les entailles entièrement à la main, l’utilisation d’un dispositif simple
dans lequel les éprouvettes sont montées et dans lequel une lame de rasoir couverte d’une pâte de diamant est
déplacée dans un mouvement alternatif à travers les éprouvettes montées présente l’avantage de pouvoir contrôler
la charge, assurer une stabilité directionnelle à la lame de rasoir et produire des entailles plus tranchantes. Un
exemple de ce dispositif est présenté dans l’Annexe A.
5.2 Pâte de diamant métallographique, dans un porteur organique visqueux et ayant une taille de
grains fins, généralement entre 1 µm et 3 µm.
5.3 Lubrifiant, une huile lubrifiante légère pour lubrifier la lame de rasoir, par exemple huile pour horloge.
5.4 Support d’éprouvettes, comprenant une plaque plane ou autre dispositif approprié destiné au
montage des éprouvettes pendant l’affûtage des entailles.
5.5 Dispositif d’essai de résistance en flexion, de préférence, un dispositif d’essai de résistance
en flexion quatre points fonctionnant conformément aux exigences de l’ISO 14704, c’est-à-dire soit en
flexion 1/4 de point (préférée) soit en flexion 1/3 de point. En variante, un montage d’essai de résistance
en flexion trois points peut aussi être utilisé, mais l’alignement de l’entaille en V avec le cylindre de charge
central est plus critique.
L’éprouvette est supportée par deux rebords portants perpendiculaires à sa longueur. Les rebords
portants externes du support doivent être des cylindres parallèles de 5,0 mm ± 0,2 mm de diamètre
et doivent être capables de rouler à l’extérieur sur des surfaces d’appui planes. De préférence, un des
cylindres doit de plus être capable de tourner autour d’un axe parallèle à la longueur de l’éprouvette de
sorte que la charge de torsion soit réduite. Les deux cylindres doivent être au départ positionnés avec
leurs centres distants de 40,0 mm ± 0,5 mm (flexion 1/4 de point) ou 30 mm ± 0,5 mm (flexion 1/3 de
2 © ISO 2012 – Tous droits réservés
point) et leurs axes parallèles à 1° environ. La séparation des centres des cylindres dans leurs positions
initiales doit être mesurée à 0,1 mm près avec un microscope mobile. Les cylindres doivent être en acier
trempé ou autre matériau dur de dureté supérieure à 40 HRC (échelle de Rockwell C). Les cylindres
doivent avoir un fini de surface lisse sans bavures avec une ténacité inférieure à 0,5 µm Ra, et avoir un
diamètre uniforme égal à ± 0,02 mm.
Pour la flexion quatre points, les deux cylindres de charge sont placés à 1/4 de point (ou 1/3 de point), avec
une portée interne de 20 mm ± 0,2 mm (ou 10 mm ± 0,2 mm pour la flexion 1/3 de point) et sont libres de
rouler à l’intérieur. Les cylindres sont libres de pivoter séparément autour d’un axe parallèle à la longueur
de l’éprouvette pour permettre l’alignement. Pour la flexion trois points, le cylindre de charge unique,
qui n’a pas besoin de pivoter, doit être positionné au centre entre les cylindres d’appui externes. Les
distances entre les cylindres doivent être mesurées à 0,1 mm près le long de la longueur de l’éprouvette
perpendiculaire à la direction de charge, à l’aide d’un microscope mobile ou autre dispositif adéquat. Les
cylindres de charge en flexion quatre points doivent être positionnés de façon symétrique à ± 0,1 mm
environ. Le dispositif de charge doit assurer que des forces identiques sont appliquées aux deux cylindres
de charge. Le cylindre de charge unique en flexion trois points doit être placé au centre à ± 0,2 mm.
5.6 Machine d’essai mécanique, capable d’appliquer une force à une vitesse constante de déplacement
ou de charge sur l’éprouvette dans le montage d’essai de résistance en flexion, et d’enregistrer la force
à laquelle la rupture de l’éprouvette survient. Le dispositif de mesure de la force doit être en conformité
avec l’ISO 7500-1 et doit avoir une exactitude ≤ 1 %.
NOTE L’équipement d’essai peut également bénéficier d’une capacité d’enregistrement de la force/du
comportement de déplacement de l’éprouvette; théoriquement il peut s’agir d’un système sensible directement
en contact avec l’éprouvette. Sous réserve d’une rigidité suffisante du train de charges, l’enregistrement du
déplacement de la machine peut être satisfaisant.
5.7 Bain de nettoyage par ultrasons, pour nettoyer les éprouvettes après entaillage, approprié pour
l’insertion d’un bécher ou autre récipient contenant du solvant.
5.8 Micromètre étalonné, similaire à celui décrit dans l’ISO 3611, mais capable d’être lu à une
résolution de 0,002 mm à l’aide d’un vernier ou d’une unité de lecture électronique.
5.9 Microscope optique, avec des grossissements étalonnés sur la plage × 50 à × 500, approprié pour
observer la forme de l’extrémité de l’entaille et muni d’équipements photo-micrographiques.
5.10 Dispositif de mesure de l’entaille, dispositif étalonné pour mesurer la profondeur de l’entaille
sciée après rupture avec une précision de lecture de 0,002 mm.
NOTE Cette profondeur peut être mesurée à l’aide d’un microscope mobile approprié ou d’un microscope
métallurgique conventionnel avec mouvement par étapes étalonné, ou d’un oculaire de réglage à micromètre étalonné.
5.11 Four de séchage, capable de maintenir une température de 120 °C ± 5 °C pour sécher les éprouvettes
après nettoyage.
5.12 Scie diamantée à refendre ou machine à refendre, capable de préparer une entaille peu profonde
dans un ensemble d’éprouvettes de 0,5 mm de large au maximum et d’une profondeur d’environ 0,5 mm.
Voir 6.3 pour des lignes directrices.
6 Préparation des éprouvettes
6.1 Nombre d’éprouvettes
Au moins sept éprouvettes doivent être préparées pour l’entaillage, dont cinq sont nécessaires pour
les essais et deux sont des éprouvettes factices destinées à la protection des cinq autres pendant la
préparation des entailles.
NOTE Si une machine est utilisée pour préparer les entailles en V, il peut ne pas être nécessaire d’utiliser les
éprouvettes factices pour protéger un banc d’essai de cinq éprouvettes.
Il est fortement recommandé aux opérateurs sans aucune expérience dans la préparation des entailles
tranchantes en V utilisées pour cette méthode de s’entraîner tout d’abord à la technique et aux matériels
avec des éprouvettes supplémentaires.
6.2 Dimensions des éprouvettes
Préparer des éprouvettes d’essai en barre de section rectangulaire, de préférence en conformité avec
les exigences de l’ISO 14704. La Figure 1 présente la forme et les dimensions principales des éprouvettes
préparées conformément à la présente Norme internationale.
NOTE 1 Les exigences de chanfreinage ou d’arrondi spécifiées dans l’ISO 14704 ne sont pas indispensables
pour l’essai des entailles en V et peuvent donc être ignorées.
NOTE 2 D’autres dimensions d’éprouvettes, par exemple (2 × 2,5 × > 25 mm) peuvent en option être utilisées
avec des dispositifs de résistance en flexion dimensionnés de manière appropriée.
Légende
L (longueur) > 45 mm (flexion 1/4 de point) ou > 35 mm (flexion 1/3 de point)
W (profondeur) 4,0 mm ± 0,2 mm
B (largeur) 3,0 mm ± 0,2 mm
Figure 1 — Dimensions de l’éprouvette conformément à l’ISO 14704
6.3 Préparation manuelle de l’entaille en V
Monter les éprouvettes côte à côte sur le support d’éprouvettes à l’aide d’un adhésif temporaire approprié,
tel qu’il est indiqué à la Figure 2. Monter les éprouvettes d’essai et les éprouvettes factices aussi proches
que possible. Veiller à ce que les faces supérieures des éprouvettes soient mises à niveau. Tracer au
4 © ISO 2012 – Tous droits réservés
crayon une ligne sur l’ensemble des éprouvettes au milieu de leur longueur, pour indiquer l’endroit où
l’entaille est à préparer. Le fléchissement des éprouvettes lors de leur montage sur le support est à éviter.
Légende
1 plaque de montage
2 éprouvettes factices
3 éprouvettes d’essai
4 ligne au crayon comme guide d’insertion d’une entaille d’amorce faite par une scie diamantée
Figure 2 — Procédure de montage de l’ensemble des éprouvettes
Monter le support sur une scie diamantée. Scier une entaille d’amorce le long du trait au crayon de
largeur ≤ 0,5 mm. Il convient que l’entaille ait la même profondeur de 0,5 mm environ sur toute sa
longueur. La Figure 3 présente un schéma du sciage. Après le sciage, nettoyer le support, les éprouvettes
et plus particulièrement l’entaille.
Dimensions en millimètres
a) Éprouvettes disposées sur le support d’éprouvettes
b) Usinage d’une entaille d’amorce avec une scie à lame diamantée mince
Légende
A surface de traction
B support
C lame de scie diamantée
D entaille sciée
X éprouvettes factices
Figure 3 — Schémas de sciage
NOTE 1 Il est utile que l’épaisseur de la lame de scie diamantée soit juste un peu plus grande que l’épaisseur
de la lame de rasoir utilisée pour l’affûtage de l’entaille. Sinon, l’extrémité de la lame de rasoir pourrait recouvrir
la surface de l’entaille pré-sciée et il pourrait être difficile de commencer le polissage de l’entaille en V. L’usinage
en V de l’extrémité de la lame de scie peut être utile lorsque les lames de scie disponibles sont sensiblement plus
épaisses que les lames de rasoir.
Fixer le support d’éprouvettes dans un étau ou autre dispositif de blocage approprié. Remplir l’entaille
d’amorce de la pâte de diamant fine, tel qu’il est présenté à la Figure 4 a).
Pour protéger les doigts, placer une lame de rasoir dans un porte-lames ou appliquer une bande
autoadhésive épaisse, tel qu’il est présenté à la Figure 4 b). Mettre la face exposée de la lame de rasoir
dans l’entaille d’amorce et exercer une force légère.
NOTE 2 Une force excessive peut être contre-productive, causant l’émoussement plus rapide de l’extrémité de
la lame de rasoir. L’application d’une force d’environ 5 N à 10 N sur la lame de rasoir pendant le polissage est
normalement suffisante.
Affûter l’entaille en V avec la lame de rasoir avec un mouvement de va et vient souple et doux [flèches
blanches à la Figure 4 b)]. Déplacer la lame de rasoir de façon aussi verticale et horizontale que possible.
NOTE 3 Une goutte d’huile lubrifiante versée sur l’entaille réduit toute saccade éventuelle ou tout coincement
éventuel de la lame de rasoir pendant l’affûtage.
6 © ISO 2012 – Tous droits réservés
a) Application de la pâte de diamant à l’aide d’une seringue sur l’entaille sciée
b) Lame de rasoir en mouvement alternatif dans l’entaille sciée
Légende
1 bande de protection épaisse
2 lame de rasoir
Figure 4 — Positionnement d’une lame de rasoir dans l’entaille sciée
Examiner périodiquement la profondeur de l’entaille en V à l’aide d’un microscope optique aux deux
extrémités de l’entaille en V. Dans toute la mesure du possible, examiner les éprouvettes sans les retirer
du porte-éprouvettes. S’il est nécessaire de les retirer et si un affûtage complémentaire est requis,
monter à nouveau les éprouvettes sur le support en insérant une lame de rasoir dans l’entaille en V pour
servir de guide. Si la profondeur totale de l’entaille en V est inférieure à 0,8 mm, poursuivre l’affûtage. Il
convient que la profondeur totale de l’entaille en V soit comprise entre 0,8 mm et 12 mm.
NOTE 4 L’affûtage manuel à l’aide d’une pâte de diamant de 4 µm produit une entaille en V de largeur S
d’environ 20 µm. L’utilisation d’une pâte de diamant plus fine, par exemple de 1 µm, ne diminue généralement pas
la largeur. Si la largeur S de l’entaille en V est supérieure à 30 µm environ, il est recommandé d’utiliser une nouvelle
lame de rasoir ou une marque différente de lame de rasoir. Pour les matériaux à gros grains, les gros grains
peuvent sauter dans l’entaille lors de l’affûtage et limiter ainsi la capacité à obtenir une entaille en V tranchante.
NOTE 5 Des matériaux différents nécessitent des périodes de temps différentes pour la préparation de l’entaille.
En général, les céramiques plus dures ou plus tenaces prennent plus de temps que les céramiques plus souples,
plus facilement usinées. Le polissage des entailles en V dans des éprouvettes d’alumine prend généralement
environ 30 min, et dans des éprouvettes de nitrure de silicium environ 4 h, pour cinq éprouvettes d’essai et deux
éprouvettes factices.
Retirer les éprouvettes du support tout en évitant de les plier. Nettoyer soigneusement les éprouvettes
avec de l’acétone dans un petit bain à ultrasons puissants. Veiller à ne pas endommager les éprouvettes
pendant le nettoyage, par exemple en leur permettant d’être en contact pendant le nettoyage par
ultrasons. Sécher les éprouvettes dans l’étuve pendant au moins 1 h à 120 °C.
NOTE 6 Le nettoyage de l’entaille en V peut être difficile, notamment lorsque le rayon de l’extrémité est petit.
Des mesures alternatives peuvent s’avérer nécessaires pour épurer ou gratter les grains de diamant.
6.4 Préparation des entailles en V à la machine (en option)
L’opération d’affûtage des entailles en V peut être automatisée. L’Annexe A présente à cet effet un exemple
de machine et les exigences principales qui s’y appliquent.
NOTE 1 Avec une machine de rigidité suffisante utilisant une pâte de diamant de 1 µm pour les phases finales
d’entaillage, la largeur de l’entaille peu
...