Abstract

This document specifies test methods of round steel hose reinforcement wire which are used for hose reinforcement. Test methods on mechanical properties and chemical properties (coating analysis) are included. By agreement, these test methods may be applied to similar single filaments used for reinforcement other rubber products.

Status
Not Published
Current Stage
6000 - International Standard under publication - 60 Publication
Start Date
31-Oct-2026

Buy Documents

Draft

ISO/FDIS 25160 - Testing method for hose reinforcement wire

Release Date:21-Aug-2026
English language (18 pages)
sale 15% off
sale 15% off
Draft

REDLINE ISO/FDIS 25160 - Testing method for hose reinforcement wire

Release Date:21-Aug-2026
English language (18 pages)
sale 15% off
sale 15% off

ISO 25160, published by ISO, specifies test methods for round steel hose reinforcement wire used for hose reinforcement. It covers mechanical property tests and coating analysis, and by agreement it may also be applied to similar single filaments used to reinforce other rubber products.

What does ISO 25160 specify?

ISO 25160 specifies how to test the diameter, tensile properties, knot strength, torsion resistance, reverse bending or flexions, cast and dead cast, and coating mass and composition of hose reinforcement wire. The document is focused on test methods, so it tells users how to measure and report results rather than how to set product requirements.

ISO 25160 is arranged in clauses 1 to 10. Clause 1 gives the scope, clause 2 lists the normative references, clause 3 defines the key terms, and clauses 4 to 10 cover the individual test methods and coating analysis procedures.

What are the key requirements of ISO 25160?

ISO 25160 sets out the test conditions and reporting rules that make results comparable between laboratories. In practice, that means specimen preparation, equipment setup, speed, temperature, and acceptance of the test run all matter as much as the final number.

Diameter measurement

Clause 4 gives two ways to measure diameter - with a micrometer or with non-contact laser methods. The micrometer route requires clean, as-straight-as-possible wire, zero-setting before each test series, and at least three readings; when ovality is needed, the method uses maximum and minimum readings rather than only an average. For laser measurement, the document requires at least 0.001 mm resolution and multiple measuring angles, which helps users capture out-of-roundness without touching the wire.

Tensile test for breaking force, yield force, and elongation

Clause 5 measures breaking force, maximum force, yield force, and elongation in a Constant-Rate-of-Extension (CRE) tensile test. The wire is clamped under defined pretension, loaded at a controlled rate, and tested until fracture, so laboratories must control grip choice, extensometer accuracy, speed, preload, and test temperature. The standard also requires rejection of results when fracture occurs too close to the grips, which matters because a grip failure does not represent the wire itself.

Knot strength

Clause 6 applies to smaller wire diameters and uses a simple overhand knot in the middle of the specimen. The knot test is a ductility check, so it is used to reveal how the wire behaves under concentrated deformation that is more severe than a straight tensile test. The procedure reduces the test speed when the knotted section reaches about 5 mm, and the report records the maximum force at fracture.

Torsion resistance

Clause 7 measures how many turns the wire can undergo in simple torsion before breaking. The specimen is held under controlled axial load, rotated at a specified speed, and the number of complete turns is counted, which helps users judge plastic deformation behavior under twisting. The clause also sets validation rules for fractures near the clamp area, because twist damage in the grip zone can invalidate the result.

Reverse bending or flexions

Clause 8 tests repeated 90° reverse bends over a cylindrical former. The wire is alternately bent left and right until fracture, so the result reflects resistance to repeated flexing rather than one-time loading. The clause includes aging options, temperature conditions, and a reporting requirement for the number of reverse bends, which is useful for comparing wire used in dynamic hose applications.

Cast and dead cast

Clause 9 measures the natural cast of the drawn wire and the tip rise, using only a smooth table and a ruler. These checks show how much the wire tends to keep a circular set or lift out of plane, which matters when the wire has to lie or feed consistently in downstream use.

Coating mass and composition

Clause 10 gives two analytical routes for brass coating - X-ray fluorescent spectrometers (XRFS) and atomic absorption spectrometry (AAS). Both routes require sample preparation, dissolution or stripping of the coating, calibration, and calculation of coating mass, composition, and thickness from measured copper and zinc values. In practice, these methods are used to verify the coating on the wire and to document the coating state in a way that can be checked by another laboratory.

What terms does ISO 25160 define?

ISO 25160 defines key force and deformation terms for interpreting test results consistently. It also uses equipment abbreviations that are important for following the procedures.

  • Breaking force - the force level at fracture, expressed in newtons.
  • Maximum force - the highest force the specimen withstands during the test, expressed in newtons.
  • Elongation - the percent total elongation at break, calculated from the extension at break relative to the original specimen length.
  • Yield force - the force level at the 0.2 % permanent elongation offset, expressed in newtons.
  • Constant-Rate-of-Extension (CRE) - a tensile testing machine that stretches the specimen at a controlled extension rate.
  • X-ray fluorescent spectrometers (XRFS) - instruments used to determine coating elemental composition from the emitted fluorescence after X-ray excitation.
  • Atomic absorption spectrometry (AAS) - an analytical method that measures copper and zinc in the dissolved coating by light absorption.

Who uses ISO 25160?

ISO 25160 is used by laboratories that test steel wire, by manufacturers of hose reinforcement wire, and by quality teams that need a repeatable way to verify wire properties. It is also relevant to hose producers, rubber-product manufacturers, and buyers who specify reinforcement wire performance in contracts or incoming inspection plans.

The document is especially useful when a team needs to compare wire from different casts, different coatings, or different suppliers. Because it covers both mechanical and coating tests, it supports production control, incoming inspection, and dispute checking using the same document.

Which standards are used with ISO 25160?

ISO 25160 refers to ISO 7800:2012 and ISO 23717. ISO 23717 provides the hose reinforcement wire terminology used in clause 3, while ISO 7800:2012 is used for torsion-related fracture characterization when that detail is requested.

These references help keep the test language and related torsion assessment aligned with other ISO documents. For users, that means the test report can point to common definitions and a recognized torsion reference method.

What does the ISO 25160 document contain?

ISO 25160 contains the test methods themselves, together with the apparatus descriptions, specimen preparation rules, and reporting statements needed to run them consistently. It includes figures for the diameter test setup, the tensile force-elongation curve, the knot test, the torsion symbols, the reverse bending equipment, and the cast and tip-rise measurements.

The document also includes formulas for diameter averaging and ovality, for tensile-derived quantities, and for coating mass, composition, and thickness. In clause 10, it provides tables for XRFS calibration standards and AAS calibration solutions, which support laboratory calibration and routine coating analysis.

Buy Documents

Draft

ISO/FDIS 25160 - Testing method for hose reinforcement wire

Release Date:21-Aug-2026
English language (18 pages)
sale 15% off
sale 15% off
Draft

REDLINE ISO/FDIS 25160 - Testing method for hose reinforcement wire

Release Date:21-Aug-2026
English language (18 pages)
sale 15% off
sale 15% off

Get Certified

Connect with accredited certification bodies for this standard

Element Materials Technology

Materials testing and product certification.

UKAS United Kingdom Verified

Inštitut za kovinske materiale in tehnologije

Institute of Metals and Technology. Materials testing, metallurgical analysis, NDT.

SA Slovenia Verified

Sponsored listings

Frequently Asked Questions

ISO 25160 is a draft published by the International Organization for Standardization (ISO). Its full title is "Testing method for hose reinforcement wire". This standard covers: This document specifies test methods of round steel hose reinforcement wire which are used for hose reinforcement. Test methods on mechanical properties and chemical properties (coating analysis) are included. By agreement, these test methods may be applied to similar single filaments used for reinforcement other rubber products.

This document specifies test methods of round steel hose reinforcement wire which are used for hose reinforcement. Test methods on mechanical properties and chemical properties (coating analysis) are included. By agreement, these test methods may be applied to similar single filaments used for reinforcement other rubber products.

ISO 25160 is classified under the following ICS (International Classification for Standards) categories: 77.140.65 - Steel wire, wire ropes and link chains. The ICS classification helps identify the subject area and facilitates finding related standards.

ISO 25160 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)

Contents

  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 3.1 breaking force
  • 3.2 maximum force
  • 3.3 elongation
  • 3.4 yield force
  • 4 Diameter
  • 4.1 Measuring with a micrometer
  • 4.2 Measuring with non-contact methods — Laser
  • 5 Breaking force and yield force and elongation
  • 5.1 Principle
  • 5.2 Apparatus
  • 5.3 Test procedure
  • 3 N for wires ≤ 0,50 mm
  • 6 Knot strength
  • 6.1 Principle
  • 6.2 Apparatus
  • 6.3 Test procedure
  • 7 Torsion resistance
  • 7.1 Principle
  • 7.2 Symbols
  • 7.3 Apparatus
  • 7.4 Test procedures
  • 8 Reverse bending or flexions
  • 8.1 Principle
  • 8.2 Apparatus
  • 8.3 Procedure
  • 9 Cast and dead cast
  • 9.1 Principle
  • 9.2 Apparatus
  • 9.3 Procedure
  • 10 Determination of mass and composition of coating
  • 10.1 Determination of mass and composition of coating by X-ray fluorescent spectrometers
  • 10.2 Determination of mass and composition of coating by atomic absorption spectrometry

1 Scope

This document specifies test methods of round steel hose reinforcement wire which are used for hose reinforcement. Test methods on mechanical properties and chemical properties (coating analysis) are included.

By agreement, these test methods can be applied to similar single filaments used for reinforcement of other rubber products.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 7800:2012, Metallic materials — Wire — Simple torsion test ISO 23717, Steel wire and wire products — Hose reinforcement wire

3 Terms and definitions

For the purposes of this document, the terms and definitions given in ISO 23717 and the following apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:

  • ISO Online browsing platform: available at https:// www .iso .org/ obp
  • IEC Electropedia: available at https:// www .electropedia .org/

3.1 breaking force

force level (B ) at fracture, expressed in N L

3.2 maximum force

F m highest force the test piece withstands, expressed in N

3.3 elongation

percent total elongation at break (A ) is the extension at break divided by the original specimen length t times 100

3.4 yield force

force level at 0,2 % permanent elongation offset, expressed in N

ISO/FDIS 25160:2026(en)

4 Diameter

4.1 Measuring with a micrometer

4.1.1 Principle

Hold a wire sample between two parallel circulars faced spindles of a micrometer. Close the movable spindle gradually with controlled speed until it is in contact with the specimen. Read the value on the micrometer.

4.1.2 Apparatus
4.1.2.1 Micrometer

a) A precision cylindrical outside micrometer with non-rotating spindle type (see Figure 1). b) In a laboratory setting, a digital precision micrometer with resolution of 0,001 mm shall be used. c) Circular spindle Φ6,35 mm d) Measuring range is from 0 mm to 25 mm.

e) Measuring force range: < 10 N.

Figure 1 — Cylindrical outside micrometer

4.1.3 Test procedure
4.1.3.1 Sample preparation

a) Cut a sample at length (about 10 cm to 15 cm).

b) A right-angle bend in the wire is to be applied to assist in rotating the wire between measurements. c) The measured area of the wire shall be as straight as possible. d) The wire surface shall be clean. Dirt and lubricant residues shall be removed with a clean tissue.

4.1.3.2 Zero-setting of the micrometer

a) Verify if the ‘display and nonius’ for digital micrometers and ‘nonius’ for analogue micrometers show 0,000 mm when the anvils are closed in a controlled way with 3 friction clicks. b) When ‘reset action’ is needed; always first clean the anvil surface of the micrometer with clean paper before the reset button is used.

c) This ‘zero-setting’ procedure needs to be done before each test series.

ISO/FDIS 25160:2026(en)

4.1.3.3 Methods of measuring

a) Method 1: Cylindrical outside micrometer: open and close method (see Figure 2).

Key d the first reading, expressed in millimetres (mm)

d is the second reading, expressed in millimetres (mm)

d is the third reading, expressed in millimetres (mm)

d is the maximum diameter, expressed in millimetres (mm) a d is the minimum diameter, expressed in millimetres (mm) b Figure 2 — Diameter test diagrams 1) The movable anvil is closed until it is in contact with the specimen. The closing speed shall be controlled until 3 clicks heard. The closing speed shall be controlled to avoid too high closing pressure and pressure overshoots.

2) Measure value 1 and record as d .

3) Measure value 2 at 60° ± 10° rotation of the wire and record as d .

4) Measure value 3 at another 60° ± 10° rotating of the wire and record as d .

NOTE 1 Avoid measuring every 90° because after 2 rotations one is measuring at same angle again. NOTE 2 When measuring method ‘out of roundness’ (ovality) is required. 5) Axially rotate the specimen between successive measurements to find maximum and minimum diameter.

b) Method 2: Cylindrical outside micrometer: rotating method (see Figure 2). 1) The movable anvil is closed until it is in contact with the specimen and stay closed under a manually applied stable closing force.

2) The sample is manually rotated 360° while the anvils are still in close position. 3) Maximum and minimum diameter is noted.

4) Average diameter is calculated out of Max and Min.

ISO/FDIS 25160:2026(en)

4.1.3.4 Calculations and report

4.1.3.4.1 Method when no ovality or out of roundness is required Determine the wire diameter by calculating the arithmetic mean of minimum 3 readings with Formula (1). d = ( d + d + d )/3 (1) 0 1 2 3 where d is the wire diameter;

st d is the 1 reading;

nd d is the 2 reading;

rd d is the 3 reading.

4.1.3.4.2 Method when ovality or out of roundness is required Determine the ‘Ovality’ by calculating the difference of the two readings with Formula (2):

O = d -d (2) v a b where d = (d + d )/2 (3) 0 a b d is the maximum diameter, expressed in millimetres (mm); a d is the minimum diameter, expressed in millimetres (mm); b d is the average diameter, expressed in millimetres (mm).

4.2 Measuring with non-contact methods — Laser

a) Resolution of 0,001 mm is minimum requirement.

b) Sample surface needs to be cleaned prior to test.

c) Sample needs to be perfect perpendicular positioned towards the laser beam. d) Sample needs to be rotatable during testing having multiple measurements to calculate average diameter or non-contact measuring devices shall be able to test in multiple angles (min 4) to take average diameter.

5 Breaking force and yield force and elongation

5.1 Principle

This test method covers the measurement of breaking force, yield force, and elongation of single filament steel reinforcement wire in a tensile test. Both ends of a test sample are clamped under a defined pretension in a tensile testing machine; increasing load under a constant rate of extension is applied until the specimen breaks. The change in force is measured versus the increase in separation of the specimen clamps to form a force-extension curve. Breaking force (load) and maximum force and percent elongation at break and yield force are measured or calculated (see Figure 3).

ISO/FDIS 25160:2026(en) Key F force e specified percentage plastic extension p 0 zero point m slope of the elastic part of the stress-percentage extension curve E e percentage extension a fracture F maximum force m A percentage total extension at fracture t Figure 3 — Tensile force - elongation curve

5.2 Apparatus

5.2.1 Tensile testing machine

a) Constant-Rate-of-Extension (CRE) tensile testing machine, its capacity shall ensure that the measured force required to fracture the wire is within the calibrated range of the loadcell. b) The capability of cross-head speed: ≥ 150 mm/min.

c) Machine accuracy Class 0,5 = Load weighing accuracy: ± 0,5 % d) Load cell capacity depends on type and characteristics of the tested wire. e) The structure of the machine and gripping systems shall be able to handle the axial force.

5.2.2 Grips

Grip types shall be selected according to the wire dimensions and wire characteristics and within the range of the load cell. They can be wedge grips type, action screw type, or pneumatic action type with suitable jaw faces (for example: smooth and ceramic or serrated jaw faces) to avoid failure of specimen at gripping point and avoid slippage of specimen within the jaws.

5.2.3 Extensometer

a) Contact or no-contact extensometer.

ISO/FDIS 25160:2026(en) b) Resolution of 0,001 % of the gauge length.

c) Standard clamp to clamp distance is 250 mm or 500 mm Standard extensometer is 200 mm.

d) Extensometer accuracy Class 05.

- Contact extensometer with sensor and contact arms - Non-contact extensometer e) Video extensometer f) Laser extensometer g) Light extensometer

5.2.4 Oven

a) An oven is required only when testing at elevated temperature is specified. b) The oven shall have a temperature capacity of at least 200 °C. c) An oven with a built-in timer is recommended.

5.3 Test procedure

5.3.1 Sample preparation

a) Sample taking process shall avoid any undulations, loops, bends or damage of the wire and wire surface. b) Cut a piece of wire of the used test length plus twice the length of a jaw face. c) When slippage occurs in the clamps, a new sample specimen shall be taken to retest. d) When requested the wire can be thermally aged in an oven. Aging time and aging temperature as agreed with requester. Standard aging conditions are: 60 min ± 1 min, at 150 °C ± 3 °C.

5.3.2 Test settings

a) Test length:

- Standard gauge length L : = 500 mm o - Standard extensometer gauge L : = 200 mm e - The gauge length L and L can be adjusted according to the requester. o e b) Speed:

- Preload speed: 5 mm/min to 15 mm/min - Test speed at 500 mm: 100 mm/min - Test speed at 250 mm: 25 mm/min - Test speed with extensometer: 20 to 60 mm/min c) Preload:

3 N for wires ≤ 0,50 mm

5 N or 10 N for wires > 0,50 mm;

ISO/FDIS 25160:2026(en) d) The preload can be adjusted the wire is not taut at preload level. - General rule: The preload shall be as low as possible, but the wire shall be taut status between the clamps, not slack.

e) The number of datapoints to construct the curve shall be at least 1 500 datapoints.

...

Contents

  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 4 Diameter
  • 4.1 Measuring with a micrometer
  • 4.2 Measuring with non-contact methods –— Laser
  • 5 Breaking force and yield force and elongation
  • 5.1 Principle
  • 5.2 Apparatus
  • 5.3 Test procedure
  • 3 N for wires ≤ 0,50 mm
  • 6 Knot strength
  • 6.1 Principle
  • 6.2 Apparatus
  • 6.3 Test procedure
  • 7 Torsion resistance
  • 7.1 Principle
  • 7.2 Symbols
  • 7.3 Apparatus
  • 7.4 Test procedures
  • 8 Reverse bending or flexions
  • 8.1 Principle
  • 8.2 Apparatus
  • 8.3 Procedure
  • 9 Cast and dead cast
  • 9.1 Principle
  • 9.2 Apparatus
  • 9.3 Procedure
  • 10 Determination of mass and composition of coating
  • 10.1 Determination of mass and composition of coating by X-ray fluorescent spectrometers
  • 10.2 Determination of mass and composition of coating by atomic absorption spectrometry

1 Scope

This document specifies test methods of round steel hose reinforcement wire which are used for hose reinforcement. Test methods on mechanical properties and chemical properties (coating analysis) are included.

By agreement, these test methods maycan be applied to similar single filaments used for reinforcement of other rubber products.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 7800:2012, Metallic materials — Wire — Simple torsion test ISO 23717, Steel wire and wire products — Hose reinforcement wire

3 Terms and definitions

For the purposes of this document, the terms and definitions given in ISO 23717 and the following apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:

  • — ISO Online browsing platform: available at https://www.iso.org/obp
  • — IEC Electropedia: available at https://www.electropedia.org/ 3.1 3.1 breaking force force level (BL) at fracture, expressed in N 3.2 3.2 maximum force F m highest force the test piece withstands, expressed in N 3.3 3.3 elongation percent total elongation at break (A ) is the extension at break divided by the original specimen length t times 100 3.4 3.4 yield force force level at 0,2 % permanent elongation offset, expressed in N

ISO/FDIS 25160:2026(en)

4 Diameter

4.1 Measuring with a micrometer

4.1.1 Principle

Hold a wire sample between two parallel circulars faced spindles of a micrometer. Close the movable spindle gradually with controlled speed until it is in contact with the specimen. Read the value on the micrometer.

4.1.2 Apparatus
4.1.2.1 Micrometer

a) a) A precision cylindrical outside micrometer with non-rotating spindle type (see Figure 1Figure 1).).

b) b) In a laboratory setting, a digital precision micrometer with resolution of 0,001 mm shall be used.

c) c) Circular spindle Φ6,35 mm d) d) Measuring range is from 0 mm to 25 mm.

e) e) Measuring force range: < 10 N.

Figure 1 — Cylindrical outside micrometer

ISO/FDIS 25160:2026(en)

4.1.3 Test procedure
4.1.3.1 Sample preparation

a) a) Cut a sample at length (about 10 cm to 15 cm).

b) b) A right-angle bend in the wire is to be applied to assist in rotating the wire between measurements.

c) c) The measured area of the wire shall be as straight as possible. d) d) The wire surface shall be clean. Dirt and lubricant residues shall be removed with a clean tissue.

4.1.3.2 Zero-setting of the micrometer

a) a) Verify if the ‘display and nonius’ for digital micrometers and ‘nonius’ for analogue micrometers show 0,000 mm when the anvils are closed in a controlled way with 3 friction clicks. b) b) When ‘reset action’ is needed; always first clean the anvil surface of the micrometer with clean paper before the reset button is used.

c) c) This ‘zero-setting’ procedure needs to be done before each test series.

4.1.3.3 Methods of measuring

a) a) Method 1: Cylindrical outside micrometer: open and close method (see Figure 2Figure 2).).

Key d1 the first reading, expressed in millimetres (mm) d is the second reading, expressed in millimetres (mm)

ISO/FDIS 25160:2026(en) d is the third reading, expressed in millimetres (mm)

da is the maximum diameter, expressed in millimetres (mm) db is the minimum diameter, expressed in millimetres (mm) Figure 2 — Diameter test diagrams 1) 1) The movable anvil is closed until it is in contact with the specimen. The closing speed shall be controlled until 3 clicks heard. The closing speed shall be controlled to avoid too high closing pressure and pressure overshoots.

2) 2) Measure value 1 and record as d1.

3) 3) Measure value 2 at 60°+/-° ± 10° rotation of the wire and record as d .

4) 4) Measure value 3 at another 60°+/-° ± 10° rotating of the wire and record as d .

NOTE 1 Avoid measuring every 90° because after 2 rotations one is measuring at same angle again. NOTE 2 When measuring method ‘out of roundness’ (ovality) is required. 5) 5) Axially rotate the specimen between successive measurements to find maximum and minimum diameter.

6) b) Method 2: Cylindrical outside micrometer: rotating method (see Figure 2Figure 2).). 1) 1) The movable anvil is closed until it is in contact with the specimen and stay closed under a manually applied stable closing force.

2) 2) The sample is manually rotated 360° while the anvils are still in close position. 3) 3) Maximum and minimum diameter is noted.

4) 4) Average diameter is calculated out of Max and Min.

4.1.3.4 Calculations and report

4.1.3.4.1 Method when no ovality or out of roundness is required Determine the wire diameter by calculating the arithmetic mean of minimum 3 readings with Formula (1)Formula (1)..

d = ( d + d + d )/3 (1) 0 1 2 3 where d is wire diameter

st d is the 1 reading

nd d is the 2 reading

rd d is the 3 reading

d is the wire diameter;

st d is the 1 reading;

nd d2 is the 2 reading;

ISO/FDIS 25160:2026(en) rd d is the 3 reading.

4.1.3.4.2 Method when ovality or out of roundness is required Determine the ‘Ovality’ by calculating the difference of the two readings with Formula (2)Formula (2):

Ov= da-db (2) where d = (d + d )/2 (3) 0 a b da is the maximum diameter, expressed in millimetres (mm)); db is the minimum diameter, expressed in millimetres (mm)); d is the average diameter, expressed in millimetres (mm)).

4.2 Measuring with non-contact methods –— Laser

a) a) Resolution of 0,001 mm is minimum requirement.

b) b) Sample surface needs to be cleaned prior to test.

c) c) Sample needs to be perfect perpendicular positioned towards the laser beam. d) d) Sample needs to be rotatable during testing having multiple measurements to calculate average diameter or non-contact measuring devices shall be able to test in multiple angles (min 4) to take average diameter.

5 Breaking force and yield force and elongation

5.1 Principle

This test method covers the measurement of breaking force, yield force, and elongation of single filament steel reinforcement wire in a tensile test. Both ends of a test sample are clamped under a defined pretension in a tensile testing machine; increasing load under a constant rate of extension is applied until the specimen breaks. The change in force is measured versus the increase in separation of the specimen clamps to form a force-extension curve. Breaking force (load) and maximum force and percent elongation at break and yield force are measured or calculated (see Figure 3Figure 3).).

ISO/FDIS 25160:2026(en)

Key F force ep specified percentage plastic extension 0 zero point mE slope of the elastic part of the stress-percentage extension curve e percentage extension a fracture F maximum force m At percentage total extension at fracture Figure 3 — Tensile force - elongation curve

ISO/FDIS 25160:2026(en)

5.2 Apparatus

5.2.1 Tensile testing machine

a) a) Constant-Rate-of-Extension (CRE) tensile testing machine, its capacity shall ensure that the measured force required to fracture the wire is within the calibrated range of the loadcell. b) b) The capability of cross-head speed: ≥ 150 mm/min.

c) c) Machine accuracy Class 0,5 = Load weighing accuracy: +/-± 0,5 % d) d) Load cell capacity depends on type and characteristics of the tested wire. e) e) The structure of the machine and gripping systems shall be able to handle the axial force.

5.2.2 Grips

Grip types shall be selected according to the wire dimensions and wire characteristics and within the range of the load cell. They can be wedge grips type, action screw type, or pneumatic action type with suitable jaw faces (for example: smooth and ceramic or serrated jaw faces) to avoid failure of specimen at gripping point and avoid slippage of specimen within the jaws.

5.2.3 Extensometer

a) a) Contact or no-contact extensometer.

b) b) Resolution of 0,001 % of the gauge length.

c) c) Standard clamp to clamp distance is 250 mm or 500 mm Standard extensometer is 200 mm.

d) d) Extensometer accuracy Class 05.

- — Contact extensometer with sensor and contact arms - — Non-contact extensometer e) e) Video extensometer f) f) Laser extensometer g) g) Light extensometer

5.2.4 Oven

a) a) An oven is required only when testing at elevated temperature is specified. b) b) The oven shall have a temperature capacity of at least 200 °C. c) c) An oven with a built-in timer is recommended.

ISO/FDIS 25160:2026(en)

5.3 Test procedure

5.3.1 Sample preparation

a) a) Sample taking process shall avoid any undulations, loops, bends or damage of the wire and wire surface.

b) b) Cut a piece of wire of the used test length plus twice the length of a jaw face. c) c) When slippage occurs in the clamps, a new sample specimen shall be taken to retest. d) d) When requested the wire can be thermally aged in an oven. Aging time and aging temperature as agreed with requester. Standard aging conditions are: 60 min ± 1 min, at 150 °C ± 3 °C.

5.3.2 Test settings

a) Test length:

- — Standard gauge length Lo: = 500 mm - — Standard extensometer gauge Le: = 200 mm - — The gauge length Lo and Le can be adjusted according to the requester. b) b) Speed:

- — Preload speed: 5 mm/min to 15 mm/min - — Test speed @at 500 mm: 100 mm/min - — Test speed @at 250 mm: 25 mm/min - — Test speed with extensometer: 20 to 60 mm/min c) c) Preload:

3 N for wires ≤ 0,50 mm

5 N or 10 N for wires > 0,50 mm; d) d) The preload can be adjusted the wire is not taut at preload level. - — General rule: The preload shall be as low as possible, but the wire shall be taut status between the clamps, not slack.

e) e) The number of datapoints to construct the curve shall be at least 15001 500 datapoints.

5.3.3 Test process

a) a) Test carried out under controlled conditions shall be made at a temperature of 23 °C +/-± 5 °C. b) b) Secure the specimen in the centre of the top clamp. Load the other end in the bottom clamp. c) c) Manually apply a pretension just below the applied pre-load to take out any residual curvature before initiating the test.

...