Standard Specification for Plates, Carbon Steel, Structural Quality, Furnished to Chemical Composition Requirements

ABSTRACT
This specification covers structural quality carbon steel plates in standard and non-standard grades furnished to chemical composition requirements. The materials shall conform to carbon, manganese, phosphorus, sulfur, silicon, and copper contents of its specified grade. Values are also given to specify the range, limit, and maximum chemical compositions of the carbon steel.
SCOPE
1.1 This specification covers structural quality carbon steel plates furnished to chemical composition requirements.  
1.2 The plates are available in several standard steel grades and non-standard grades.  
1.3 The plates are usually furnished in the as-rolled (hot-rolled) condition.  
1.4 Supplementary requirements are provided for additional requirements that may be specified on the order.  
1.5 When the steel is to be welded, it is presupposed that a welding procedure suitable for the grade of steel and intended use or service will be utilized. See Appendix X3 of Specification A6/A6M for information on weldability.  
1.6 The values stated in either SI units or inch-pound units are to be regarded separately as standard. The values stated in each system may not be exact equivalents; therefore, each system shall be used independently of the other. Combining values from the two systems may result in non-conformance with the standard.

General Information

Status
Historical
Publication Date
30-Apr-2014
Current Stage
Ref Project

Relations

Buy Standard

Technical specification
ASTM A830/A830M-14 - Standard Specification for Plates, Carbon Steel, Structural Quality, Furnished to Chemical Composition Requirements
English language
4 pages
sale 15% off
Preview
sale 15% off
Preview
Technical specification
REDLINE ASTM A830/A830M-14 - Standard Specification for Plates, Carbon Steel, Structural Quality, Furnished to Chemical Composition Requirements
English language
4 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation:A830/A830M −14
Standard Specification for
Plates, Carbon Steel, Structural Quality, Furnished to
1
Chemical Composition Requirements
This standard is issued under the fixed designationA830/A830M; the number immediately following the designation indicates the year
of original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval.
A superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope* A6/A6M Specification for General Requirements for Rolled
Structural Steel Bars, Plates, Shapes, and Sheet Piling
1.1 This specification covers structural quality carbon steel
plates furnished to chemical composition requirements.
3. Ordering Information
1.2 The plates are available in several standard steel grades
3.1 In addition to the information required by Specification
and non-standard grades.
A6/A6M, the order shall include the following, if applicable:
3.1.1 Silicon requirements (see 5.3 and Supplementary Re-
1.3 The plates are usually furnished in the as-rolled (hot-
quirement S96), and
rolled) condition.
3.1.2 Limitation on rimmed or capped steel.
1.4 Supplementary requirements are provided for additional
4. Materials and Manufacture
requirements that may be specified on the order.
1.5 When the steel is to be welded, it is presupposed that a 4.1 The steel shall be killed.
welding procedure suitable for the grade of steel and intended
5. Chemical Composition
use or service will be utilized. See Appendix X3 of Specifica-
5.1 The heat analysis shall conform to the requirements for
tion A6/A6M for information on weldability.
the applicable grade listed in Table 1, unless otherwise speci-
1.6 The values stated in either SI units or inch-pound units
fied as permitted in 5.2.
are to be regarded separately as standard. The values stated in
5.2 The chemical requirements for heat analysis may be
each system may not be exact equivalents; therefore, each
specified in accordance with the ranges and limits listed in
system shall be used independently of the other. Combining
Table 2. In such instances, the heat analysis shall conform to
values from the two systems may result in non-conformance
the requirements specified on the order.
with the standard.
5.3 Whensiliconisrequired,therangeonheatanalysisshall
2. Referenced Documents
be from 0.15 to 0.40 % unless otherwise specified on the order
2
2.1 ASTM Standards: (see Supplementary Requirement S96).
6. General Requirements
1
This specification is under the jurisdiction ofASTM Committee A01 on Steel,
6.1 Material furnished under this specification shall con-
Stainless Steel and Related Alloys and is the direct responsibility of Subcommittee
form to the requirements of the current edition of Specification
A01.02 on Structural Steel for Bridges, Buildings, Rolling Stock and Ships.
A6/A6M, for the ordered material, unless a conflict exists in
Current edition approved May 1, 2014. Published May 2014. Originally
approved in 1984. Last previous edition approved in 2013 as A830/A830M – 13.
which case this specification shall prevail.
DOI: 10.1520/A0830_A0830M-14.
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or 7. Keywords
contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM
7.1 carbon; chemical composition; non-standard grades;
Standards volume information, refer to the standard’s Document Summary page on
the ASTM website. plates; standard grades; steel; structural steel
*A Summary of Changes section appears at the end of this standard
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
A830/A830M−14
A
TABLE 1 Carbon Plate Compositions, Standard Steels
Grade Chemical Composition Limits, %
Number Carbon Manganese Phosphorous, max Sulfur, max
1006 0.08 max 0.45 max 0.030 0.030
1008 0.10 max 0.50 max 0.030 0.030
1009 0.15 max 0.60 max 0.030 0.030
1010 0.08 to 0.13 0.30 to 0.60 0.030 0.030
1012 0.10 to 0.15 0.30 to 0.60 0.030 0.030
1015 0.13 to 0.18 0.30 to 0.60 0.030 0.030
1016 0.13 to 0.18 0.60 to 0.90 0.030 0.030
1017 0.15 to 0.20 0.30 to 0.60 0.030 0.030
1018 0.15 to 0.20 0.60 to 0.90 0.030 0.030
1019 0.15 to 0.20 0.70 to 1.00 0.030 0.030
1020 0.18 to 0.23 0.30 to 0.60 0.030 0.030
1021 0.18 to 0.23 0.60 to 0.90 0.030 0.030
1022 0.18 to 0.23 0.70 to 1.00 0.030 0.030
1023 0.20 to 0.25 0.30 to 0.60 0.030 0.030
1025 0.22 to 0.28 0.30 to 0.60 0.030 0.030
1026 0.22 to 0.28 0.60 to 0.90 0.030 0.030
1030 0.28 to 0.34 0.60 to 0.90 0.030 0.030
1033 0.30 to 0.36 0.70 to 1.00 0.030 0.030
1035 0.32 to 0.38 0.60 to 0.90 0.030 0.030
1037 0.32 to 0.38 0.70 to 1.00 0.030 0.030
1038 0.35 to 0.42 0.60 to 0.90 0.030 0.030
1039 0.37 to 0.44 0.70 to 1.00 0.030 0.030
104
...

This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
Designation: A830/A830M − 13 A830/A830M − 14
Standard Specification for
Plates, Carbon Steel, Structural Quality, Furnished to
1
Chemical Composition Requirements
This standard is issued under the fixed designation A830/A830M; the number immediately following the designation indicates the year
of original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval.
A superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope*
1.1 This specification covers structural quality carbon steel plates furnished to chemical composition requirements.
1.2 The plates are available in several standard steel grades and non-standard grades.
1.3 The plates are usually furnished in the as-rolled (hot-rolled) condition.
1.4 Supplementary requirements are provided for additional requirements that may be specified on the order.
1.5 When the steel is to be welded, it is presupposed that a welding procedure suitable for the grade of steel and intended use
or service will be utilized. See Appendix X3 of Specification A6/A6M for information on weldability.
1.6 The values stated in either SI units or inch-pound units are to be regarded separately as standard. The values stated in each
system may not be exact equivalents; therefore, each system shall be used independently of the other. Combining values from the
two systems may result in non-conformance with the standard.
2. Referenced Documents
2
2.1 ASTM Standards:
A6/A6M Specification for General Requirements for Rolled Structural Steel Bars, Plates, Shapes, and Sheet Piling
3. Ordering Information
3.1 In addition to the information required by Specification A6/A6M, the order shall include the following, if applicable:
3.1.1 Silicon requirements (see 5.3 and Supplementary Requirement S96), and
3.1.2 Limitation on rimmed or capped steel.
4. Materials and Manufacture
4.1 The steel shall be killed.
5. Chemical Composition
5.1 The heat analysis shall conform to the requirements for the applicable grade listed in Table 1, unless otherwise specified as
permitted in 5.2.
5.2 The chemical requirements for heat analysis may be specified in accordance with the ranges and limits listed in Table 2. In
such instances, the heat analysis shall conform to the requirements specified on the order.
5.3 When silicon is required, the range on heat analysis shall be from 0.15 to 0.40 % unless otherwise specified on the order
(see Supplementary Requirement S96).
6. General Requirements
6.1 Material furnished under this specification shall conform to the requirements of the current edition of Specification
A6/A6M, for the ordered material, unless a conflict exists in which case this specification shall prevail.
1
This specification is under the jurisdiction of ASTM Committee A01 on Steel, Stainless Steel and Related Alloys and is the direct responsibility of Subcommittee A01.02
on Structural Steel for Bridges, Buildings, Rolling Stock and Ships.
Current edition approved May 1, 2013May 1, 2014. Published June 2013May 2014. Originally approved in 1984. Last previous edition approved in 20112013 as
A830/A830M – 11.A830/A830M – 13. DOI: 10.1520/A0830_A0830M-13.10.1520/A0830_A0830M-14.
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards
volume information, refer to the standard’s Document Summary page on the ASTM website.
*A Summary of Changes section appears at the end of this standard
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
A830/A830M − 14
A
TABLE 1 Carbon Plate Compositions, Standard Steels
Grade Chemical Composition Limits, %
Number Carbon Manganese Phosphorous, max Sulfur, max
1006 0.08 max 0.45 max 0.035 0.04
1006 0.08 max 0.45 max 0.030 0.030
1008 0.10 max 0.50 max 0.035 0.04
1008 0.10 max 0.50 max 0.030 0.030
1009 0.15 max 0.60 max 0.035 0.04
1009 0.15 max 0.60 max 0.030 0.030
1010 0.08 to 0.13 0.30 to 0.60 0.035 0.04
1010 0.08 to 0.13 0.30 to 0.60 0.030 0.030
1012 0.10 to 0.15 0.30 to 0.60 0.035 0.04
1012 0.10 to 0.15 0.30 to 0.60 0.030 0.030
1015 0.13 to 0.18 0.30 to 0.60 0.035 0.04
1015 0.13 to 0.18 0.30 to 0.60 0.030 0.030
1016 0.13 to 0.18 0.60 to 0.90 0.035 0.04
1016 0.13 to 0.18 0.60 to 0.90 0.030 0.030
1017 0.15 to 0.20 0.30 to 0.60 0.035 0.04
1017 0.15 to 0.20 0.30 to 0.60 0.030 0.030
1018 0.15 to 0.20 0.60 to 0.90 0.035 0.04
10
...

Questions, Comments and Discussion