Standard Test Method for Fineness of Dispersion of Pigment-Vehicle Systems by Hegman-Type Gage

SIGNIFICANCE AND USE
4.1 In making pigmented products, the pigment is usually dispersed in a portion of the vehicle in some sort of mill. At this stage, it is necessary to be able to judge if the pigment agglomerates have been sufficiently broken up so as not to interfere with the smoothness of the finished coating film. This test method describes a way of making this judgment.
SCOPE
1.1 This test method covers measurement of the degree of dispersion (commonly referred to as “fineness of grind”) of the pigment in a pigment-vehicle system such as liquid coatings and their intermediates. It may also be used to assess the inclusion of particulates by a cleanliness (or texture) rating.  
1.2 The values stated in SI units are to be regarded as the standard. The values given in parentheses are for information only.  
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.

General Information

Status
Historical
Publication Date
30-Nov-2014
Current Stage
Ref Project

Buy Standard

Standard
ASTM D1210-05(2014) - Standard Test Method for Fineness of Dispersion of Pigment-Vehicle Systems by Hegman-Type Gage
English language
11 pages
sale 15% off
Preview
sale 15% off
Preview
Standard
REDLINE ASTM D1210-05(2014) - Standard Test Method for Fineness of Dispersion of Pigment-Vehicle Systems by Hegman-Type Gage
English language
11 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)

NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D1210 − 05 (Reapproved 2014)
Standard Test Method for
Fineness of Dispersion of Pigment-Vehicle Systems by
1
Hegman-Type Gage
This standard is issued under the fixed designation D1210; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the U.S. Department of Defense.
2 2
1. Scope this gage, each of 6.5 cm (1 in. ) area, and of two different
depths. A count is made of the particles deposited in the two
1.1 This test method covers measurement of the degree of
delimited areas, and cleanliness (texture) reading is deter-
dispersion (commonly referred to as “fineness of grind”) of the
mined.
pigment in a pigment-vehicle system such as liquid coatings
and their intermediates. It may also be used to assess the
4. Significance and Use
inclusion of particulates by a cleanliness (or texture) rating.
4.1 In making pigmented products, the pigment is usually
1.2 The values stated in SI units are to be regarded as the
dispersedinaportionofthevehicleinsomesortofmill.Atthis
standard. The values given in parentheses are for information
stage, it is necessary to be able to judge if the pigment
only.
agglomerates have been sufficiently broken up so as not to
1.3 This standard does not purport to address all of the
interfere with the smoothness of the finished coating film. This
safety concerns, if any, associated with its use. It is the
test method describes a way of making this judgment.
responsibility of the user of this standard to establish appro-
5. Apparatus
priate safety and health practices and determine the applica-
bility of regulatory limitations prior to use.
5.1 Tapered Gage—A hardened steel, stainless steel, or
chrome-plated steel block (Fig. 1) approximately 170 mm (6.7
2. Referenced Documents
in.) in length, and 15 mm (0.6 in.) in thickness.The top surface
2
of the block shall be ground smooth and planar and shall
2.1 ASTM Standards:
D1316 Test Method for Fineness of Grind of Printing Inks contain one or two paths 127 mm (5 in.) in calibrated length.
The path shall be tapered uniformly in depth lengthwise from
By the NPIRI Grindometer
about 4 mils (100 µm) at 10 mm from one end to zero depth at
3. Summary of Test Method
the other with intermediate calibrations in accordance with the
depth at those points. Preferred calibrations are Hegman units
3.1 Tapered Gage—The product is spread by means of a
and micrometers (Note 1). Three path widths are covered by
scraper in a machined tapered path.At some point in this path,
this test method:
particlesoragglomerates,orboth,willbecomevisible.Adirect
5.1.1 Two Parallel Paths, each 12.5-mm (0.5-in.) wide and
reading from the graduated scale is then made at the point
spaced 0.5-in. apart centered in a block 65-mm (2.5-in.) wide
where the particles form a definite pattern. When the single
(see Fig. 1).
path gage is used it is also possible to rate “cleanliness” (see
5.1.2 One Path, 50 mm (2 in.) in width centered in a block
6.2).
90-mm (3.5-in.) wide (see Fig. 1).
3.2 Stepped Gage—The product is spread by means of a
5.1.3 One Path, 25 mm (1 in.) in width centered in a block
scraper on a stepped gage. There are 2 delimited sections on
65-mm (2.5-in.) wide (see Fig. 1a).
NOTE1—Severalarbitraryscalesandmodificationsofthegageareused
1 by industry. In order that readings obtained with these arbitrary scales and
This test method is under the jurisdiction of ASTM Committee D01 on Paint
modifications can be reported in the preferred units, the approximate
and Related Coatings, Materials, andApplications and is the direct responsibility of
relationship of these scales to gage depth is shown in the following
Subcommittee D01.24 on Physical Properties of Liquid Paints and Paint Materials.
example:
Current edition approved Dec. 1, 2014. Published December 2014. Originally
approved in 1952. Last previous edition approved in 2010 as D1210 – 05 (2010).
DOI: 10.1520/D1210-05R14.
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or
contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM
Standards volume information, refer to the standard’s Document Summary page on
the ASTM website.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
D1210 − 05 (2014)
FIG. 1 Fineness Gages
the seller. There shall be two tick marks, above and below the
Hegman Depth, Depth, PC or FSPT NPIRI
A B B C D
Scale µm mils Scale Scale
“step,” and spaced 25 mm (1 in.) from it.
0 100 4 0 40
1
1
...

This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
Designation: D1210 − 05 (Reapproved 2010) D1210 − 05 (Reapproved 2014)
Standard Test Method for
Fineness of Dispersion of Pigment-Vehicle Systems by
1
Hegman-Type Gage
This standard is issued under the fixed designation D1210; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the U.S. Department of Defense.
1. Scope
1.1 This test method covers measurement of the degree of dispersion (commonly referred to as “fineness of grind”) of the
pigment in a pigment-vehicle system such as liquid coatings and their intermediates. It may also be used to assess the inclusion
of particulates by a cleanliness (or texture) rating.
1.2 The values stated in SI units are to be regarded as the standard. The values given in parentheses are for information only.
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility
of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory
limitations prior to use.
2. Referenced Documents
2
2.1 ASTM Standards:
D1316 Test Method for Fineness of Grind of Printing Inks By the NPIRI Grindometer
3. Summary of Test Method
3.1 Tapered Gage—The product is spread by means of a scraper in a machined tapered path. At some point in this path, particles
or agglomerates, or both, will become visible. A direct reading from the graduated scale is then made at the point where the
particles form a definite pattern. When the single path gage is used it is also possible to rate “cleanliness” (see 6.2).
3.2 Stepped Gage—The product is spread by means of a scraper on a stepped gage. There are 2 delimited sections on this gage,
2 2
each of 6.5 cm (1 in. ) area, and of two different depths. A count is made of the particles deposited in the two delimited areas,
and cleanliness (texture) reading is determined.
4. Significance and Use
4.1 In making pigmented products, the pigment is usually dispersed in a portion of the vehicle in some sort of mill. At this stage,
it is necessary to be able to judge if the pigment agglomerates have been sufficiently broken up so as not to interfere with the
smoothness of the finished coating film. This test method describes a way of making this judgment.
5. Apparatus
5.1 Tapered Gage—A hardened steel, stainless steel, or chrome-plated steel block (Fig. 1) approximately 170 mm (6.7 in.) in
length, and 15 mm (0.6 in.) in thickness. The top surface of the block shall be ground smooth and planar and shall contain one
or two paths 127 mm (5 in.) in calibrated length. The path shall be tapered uniformly in depth lengthwise from about 4 mils (100
μm) at 10 mm from one end to zero depth at the other with intermediate calibrations in accordance with the depth at those points.
Preferred calibrations are Hegman units and micrometers (Note 1). Three path widths are covered by this test method:
5.1.1 Two Parallel Paths, each 12.5-mm (0.5-in.) wide and spaced 0.5-in. apart centered in a block 65-mm (2.5-in.) wide (see
Fig. 1).
1
This test method is under the jurisdiction of ASTM Committee D01 on Paint and Related Coatings, Materials, and Applications and is the direct responsibility of
Subcommittee D01.24 on Physical Properties of Liquid Paints &and Paint Materials.
Current edition approved Feb. 1, 2010Dec. 1, 2014. Published February 2010December 2014. Originally approved in 1952. Last previous edition approved in 20052010
as D1210 – 05.D1210 – 05 (2010). DOI: 10.1520/D1210-05R10.10.1520/D1210-05R14.
2
For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards
volume information, refer to the standard’sstandard’s Document Summary page on the ASTM website.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1

---------------------- Page: 1 ----------------------
D1210 − 05 (2014)
FIG. 1 Fineness Gages
5.1.2 One Path, 50 mm (2 in.) in width centered in a block 90-mm (3.5-in.) wide (see Fig. 1).
5.1.3 One Path, 25 mm (1 in.) in width centered in a block 65-mm (2.5-in.) wide (see Fig. 1a).
NOTE 1—Several arbitrary scales and modifications of the gage are used by industry
...

Questions, Comments and Discussion

Ask us and Technical Secretary will try to provide an answer. You can facilitate discussion about the standard in here.