oSIST prEN 196-1:2026
(Main)Methods of testing cement - Part 1: Determination of strength
- Abstract
This part of EN 196 describes the method for the determination of the compressive and, optionally, the flexural strength of cement mortar. The method applies to common cements and to other cements and materials, the standards for which call up this method. It may not apply to other cement types that have, for example, a very short initial setting time.
The method is used for assessing whether the compressive strength of cement is in conformity with its specification and for validation testing of a CEN Standard sand, EN 196 1, or alternative compaction equipment.
This part of EN 196 describes the reference equipment and procedure and allows alternative compaction equipment and procedures to be used provided that they have been validated in accordance with the appropriate provisions in this document. In the event of a dispute, only the reference equipment and procedure are used.
- Status
- Not Published
- Public Enquiry End Date
- 22-Oct-2026
- Technical Committee
- CAA - Mineral binders and masonry
- Current Stage
- 4020 - Public enquire (PE) (Adopted Project)
- Start Date
- 06-Aug-2026
- Due Date
- 24-Dec-2026
oSIST prEN 196-1:2026 is the Slovenian draft standard published by SIST for CEN draft prEN 196-1. It specifies the reference method for determining the compressive strength of cement mortar, and optionally its flexural strength, for common cements and for other cements or materials that call up this method. It is intended for laboratories, cement producers, and certification bodies that need a common procedure for conformity assessment, CEN Standard sand validation, or validation of alternative compaction equipment.
What does oSIST prEN 196-1:2026 specify?
oSIST prEN 196-1:2026 specifies the equipment and procedure for preparing, curing, and testing standard mortar made with cement, CEN Standard sand, and water. It also sets the characteristics of CEN Reference sand and the minimum requirements and acceptance procedure for CEN Standard sand.
The document covers the full test chain: laboratory conditions, equipment, mortar constituents, specimen preparation, conditioning, strength testing, result calculation, and validation testing. In dispute, only the reference equipment and procedure, or the reference sand, are to be used.
Its structure is practical and test-driven. Clause 1 gives the scope, Clauses 2 to 11 cover the method itself, Clause 12 covers validation of CEN Standard sand and alternative compaction equipment, and normative Annex A lists validated alternative vibration compaction equipment and procedures.
What are the key requirements of oSIST prEN 196-1:2026?
Mortar, specimens, and basic method
The test uses prismatic specimens of 40 mm × 40 mm × 160 mm made from mortar with one part cement, three parts CEN Standard sand, and one-half part water. For a normal batch of three prisms, the document gives the batch quantities and requires mechanical mixing. In practice, this keeps results comparable between laboratories and between cement products.
The mortar is compacted in moulds using the reference jolting apparatus, unless a validated alternative compaction method is used. The method also allows flexural strength to be measured first, followed by compressive strength on the broken halves. That means the same prisms can provide both values when required.
Laboratory conditions and equipment control
The laboratory, moist air room or cabinet, and water-curing containers are held at controlled temperatures, and the room humidity is also controlled. The document requires temperature and humidity records during working hours, and more frequent checks for the moist air room or cabinet. This matters because cement strength development is sensitive to storage conditions.
Clause 5 sets detailed requirements for the mixer, moulds, jolting apparatus, flexural strength testing apparatus, compressive strength testing machine, jig, balance, and timer. The document also says that critical tolerances must be respected, and that equipment should be rejected, adjusted, or repaired if control measurements show it is out of tolerance. For the user, that means equipment condition is part of the method, not just a maintenance issue.
Sand and water requirements
Clause 6 distinguishes between the CEN Reference sand and CEN Standard sand. CEN Standard sand is the normal test sand, but it must meet the particle size distribution and moisture limits and must also be validated against the CEN Reference sand. The sand producer is responsible for certification and ongoing verification testing.
For water, distilled or deionized water is required for validation testing, while drinking water is allowed for other tests unless there is a dispute. This gives a clear rule for routine work versus formal validation work.
Specimen preparation, curing, and test ages
Clause 8 requires immediate moulding after mortar preparation, with two layers compacted separately and 60 jolts for each layer. Clause 9 then requires moist storage in the mould for 24 h, careful demoulding, and curing under water at controlled temperature. The specimens are tested at specified ages, including 24 h, 48 h, 72 h, 7 d, and 28 d within stated time windows.
In practice, the timing rules are important because the test age is measured from the defined zero time in the mixing procedure. Any delay in demoulding has to be recorded. That helps users explain result differences if curing or handling was not normal.
Strength testing and result treatment
Clause 10 gives the flexural and compressive testing procedures. Flexural strength uses three-point loading with a defined loading rate, while compressive strength is measured on the prism halves at a separate loading rate. The machine alignment, platen condition, and centring requirements reduce false results caused by uneven loading.
Clause 11 explains how to calculate and report the results. Flexural strength is the arithmetic mean of three results, and compressive strength is the arithmetic mean of six results from three prisms. There is also a rule for discarding one result if it differs too much from the mean, and then repeating the determination if needed. For quality control, this gives a clear rule for outlier handling and reporting.
Clause 11.2.3 gives precision information for compressive strength in terms of short-term repeatability, long-term repeatability, and reproducibility. Those precision statements are used when laboratories check their own performance, compare results, or judge conformity.
Validation of sand and alternative compaction equipment
Clause 12 sets the validation scheme for CEN Standard sand and alternative compaction equipment. Validation is based on 28 d compressive strength comparisons against the CEN Reference sand or the reference jolting apparatus, with results assessed by the validation criterion D. The document requires the validation criterion to stay below 5.0 % in the stated tests.
For CEN Standard sand, the procedure includes certification testing and ongoing verification testing by the producer under the authority of a certification body. For alternative compaction equipment, the producer or applicant must supply a full technical description, and the equipment is compared with the reference jolting apparatus in a certification-body-controlled test programme. In practice, this is the route for proving that a non-reference compaction system is acceptable.
What changed in oSIST prEN 196-1:2026 from the previous edition?
oSIST prEN 196-1:2026 will supersede EN 196-1:2016. The foreword states two significant changes:
- a revised procedure for adding water to the containers in 9.3
- limits for clay content and water-soluble chloride in standard sand during initial certification testing in 12.2.2.1
These changes matter because they affect curing practice and the acceptance of CEN Standard sand at the certification stage.
Who uses oSIST prEN 196-1:2026?
This standard is used by cement laboratories, cement producers, and certification bodies. It supports routine conformity testing of cement strength, validation of CEN Standard sand, and validation of alternative compaction equipment.
Quality managers use it to define accepted test conditions, control precision, and review whether results are comparable across sites or suppliers. Buyers and specifiers can use it to understand how compressive strength values are generated and what method lies behind the declared results.
Which standards are used with oSIST prEN 196-1:2026?
| Standard | What it contributes |
|---|---|
| EN 196-7 | Sampling and preparation of cement samples before testing |
| EN 197-1 | Common cement categories used in the scope and validation work |
| EN 1744-1 | Measurement of water-soluble chlorides in sand |
| EN ISO 1302 | Surface texture notation for equipment surfaces |
| EN ISO 7500-1 | Verification of the force-measuring system of the compression machine |
| ISO 565 | Nominal sieve opening sizes |
| ISO 1101 | Geometrical tolerancing for flatness and perpendicularity |
| ISO 3310-1 | Technical requirements for test sieves |
| ISO 4200 | Tube sizes used for jolting apparatus arms |
| EN 933-9 | Methylene blue test used for clay and fine substances in sand validation |
What does the oSIST prEN 196-1:2026 document contain?
The document contains the full test method, including laboratory control conditions, equipment requirements, mortar composition, mixing, moulding, curing, flexural testing, compressive testing, result calculation, reporting, and validation. It includes tables for sieve apertures, mixer speeds, and reference sand grading.
It also contains detailed figures for the mixer, mould, jolting apparatus, flexural loading arrangement, compressive jig, and alternative vibrating tables. Formulae are provided for flexural strength, compressive strength, and the validation criterion used for sand and equipment comparison.
Annex A gives the technical descriptions and compaction procedures for validated alternative vibration compaction equipment. For users, this annex is the practical reference for choosing a validated alternative to the jolting method.
Relations
- Effective Date
- 28-Jan-2023
Get Certified
Connect with accredited certification bodies for this standard

DIBt (Deutsches Institut für Bautechnik)
German Institute for Building Technology.
DIN CERTCO
DIN Group product certification.

Aboma Certification B.V.
Specialized in construction, metal, and transport sectors.
Sponsored listings
Frequently Asked Questions
oSIST prEN 196-1:2026 is a draft published by the Slovenian Institute for Standardization (SIST). Its full title is "Methods of testing cement - Part 1: Determination of strength". This standard covers: This part of EN 196 describes the method for the determination of the compressive and, optionally, the flexural strength of cement mortar. The method applies to common cements and to other cements and materials, the standards for which call up this method. It may not apply to other cement types that have, for example, a very short initial setting time. The method is used for assessing whether the compressive strength of cement is in conformity with its specification and for validation testing of a CEN Standard sand, EN 196 1, or alternative compaction equipment. This part of EN 196 describes the reference equipment and procedure and allows alternative compaction equipment and procedures to be used provided that they have been validated in accordance with the appropriate provisions in this document. In the event of a dispute, only the reference equipment and procedure are used.
This part of EN 196 describes the method for the determination of the compressive and, optionally, the flexural strength of cement mortar. The method applies to common cements and to other cements and materials, the standards for which call up this method. It may not apply to other cement types that have, for example, a very short initial setting time. The method is used for assessing whether the compressive strength of cement is in conformity with its specification and for validation testing of a CEN Standard sand, EN 196 1, or alternative compaction equipment. This part of EN 196 describes the reference equipment and procedure and allows alternative compaction equipment and procedures to be used provided that they have been validated in accordance with the appropriate provisions in this document. In the event of a dispute, only the reference equipment and procedure are used.
oSIST prEN 196-1:2026 is classified under the following ICS (International Classification for Standards) categories: 91.100.10 - Cement. Gypsum. Lime. Mortar. The ICS classification helps identify the subject area and facilitates finding related standards.
oSIST prEN 196-1:2026 has the following relationships with other standards: It is inter standard links to SIST EN 196-1:2016. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.
oSIST prEN 196-1:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 4 Principle
- 5 Laboratory and equipment
- 5.1 Laboratory
- 5.2 General requirements for the equipment
- 5.3 Test sieves
- 5.4 Mixer
- 5.5 Moulds
- 5.6 Jolting apparatus
- 5.7 Flexural strength testing apparatus
- 5.8 Compressive strength testing machine
- 5.9 Jig for compressive strength testing machine
- 5.10 Balance
- 5.11 Timer
- 6 Mortar constituents
- 6.1 Sand
- 6.2 Cement
- 6.3 Water
- 7 Preparation of mortar
- 7.1 Composition of mortar
- 7.2 Mixing of mortar
- 8 Preparation of test specimens
- 8.1 Size of specimens
- 8.2 Moulding of test specimens
- 9 Conditioning of test specimens
- 9.1 Handling and storage before demoulding
- 9.2 Demoulding of specimens
- 9.3 Curing of specimens in water
- 9.4 Age of specimens for strength tests
- 10 Testing procedures
- 10.1 Flexural strength
- 10.2 Compressive strength
- 11 Results
- 11.1 Flexural strength
- 11.2 Compressive strength
- 12 Validation testing of CEN Standard sand and of alternative compaction
- 12.1 General
- 12.2 Validation testing of CEN Standard sand
- 12.3 Validation testing of alternative compaction equipment
- Annex A
- Bibliography
1 Scope
This document specifies the equipment and procedure for the preparation and curing of a standard mortar to be used for the determination of the compressive and flexural strength of a common cement in accordance with EN 197-1.
The determination of compressive or flexural strength can be carried out at different curing ages. The document also describes an alternative method for the compaction of the standard mortar, which can be considered equivalent.
In addition, the document specifies the characteristics of a CEN reference sand and the minimum requirement and the acceptance procedure for the CEN standard sand. In the case of a dispute, only the reference methods or reference sand can be used. The same equipment and procedures can be used for other types of cement or materials; in some cases, modifications to the procedure are also permitted, provided that this standard and/or the modifications are referenced in the relevant product standards.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. EN 196-7, Methods of testing cement — Methods of taking and preparing samples of cement EN 197-1, Cement — Part 1: Composition, specifications and conformity criteria for common cements EN 1744-1, Tests for chemical properties properties of aggregates - Part 9: Chemical analysis EN ISO 1302, Geometrical Product Specifications (GPS) — Indication of surface texture in technical product documentation (ISO 1302:2002) EN ISO 7500-1, Metallic materials — Verification of static uniaxial testing machines — Part 1:
Tension/compression testing machines - Verification and calibration of the force-measuring system (ISO 7500-1:2004) ISO 565, Test sieves — Metal wire cloth, perforated metal plate and electroformed sheet — Nominal sizes of openings ISO 1101, Geometrical Product Specifications (GPS) — Geometrical tolerancing — Tolerances of form, orientation, location and run-out ISO 3310-1, Test sieves — Technical requirements and testing — Part 1: Test sieves of metal wire cloth ISO 4200, Plain end steel tubes, welded and seamless; general tables of dimensions and masses per unit length
3 Terms and definitions
No terms and definitions are listed in this document.
4 Principle
The method comprises the determination of the compressive, and optionally the flexural, strength of prismatic test specimens 40 mm × 40 mm × 160 mm in size.
oSIST prEN 196-1:2026 prEN 196-1 (E) These specimens are cast from a batch of plastic mortar containing one part by mass of cement, three parts by mass of CEN Standard sand and one half part of water (water/cement ratio 0,50). CEN Standard sands from various sources and countries may be used provided that they have been shown to give cement strength results which do not differ significantly from those obtained using the CEN Reference sand (see Clause 11).
In the reference procedure the mortar is prepared by mechanical mixing and is compacted in a mould using a jolting apparatus. Alternative compaction equipment and procedures may be used provided that they have been shown to give cement strength results which do not differ significantly from those obtained using the reference jolting apparatus and procedure (see Clause 11 and Annex A ). The specimens are stored in the mould in a moist atmosphere for 24 h and, after demoulding, specimens are stored under water until strength testing.
At the required age, the specimens are taken from their wet storage, broken in flexure, determining the flexural strength where required, or broken using other suitable means which do not subject the prism halves to harmful stresses, and each half tested for strength in compression.
5 Laboratory and equipment
5.1 Laboratory
The laboratory where preparation of specimens takes place shall be maintained at a temperature of (20 ± 2) °C and a relative humidity of not less than 50 %.
The moist air room or the large cabinet for storage of the specimens in the mould shall be maintained at a temperature of (20,0 ± 1,0) °C and a relative humidity of not less than 90 %. NOTE 1 If the moulds are stored in a cabinet and sealed with grease, preventing any evaporation, it is sufficient to store an open water reservoir in the basement of the cabinet. NOTE 2 The cabinet is a lockable cupboard or box in which the moulds are stored; it is usually kept closed and only opened for storing or removing moulds The storage containers for curing the specimens in water, and the grates with which they are fitted, shall be of material which does not react with cement. The temperature of the water shall be maintained at (20,0 ± 1,0) °C.
The temperature and relative humidity of the air in the laboratory and the temperature of the water in the storage containers shall be recorded at least once a day during working hours. The temperature and relative humidity of the moist air room or cabinet shall be recorded at least every 4 h. Cement, CEN Standard sand (see 6.1.3), water and apparatus used to make and test specimens shall be at a temperature of (20 ± 2) °C.
Where temperature ranges are given, the target temperature at which the controls are set shall be the middle value of the range.
5.2 General requirements for the equipment
The tolerances shown in Figure 1 to Figure 5 are important for correct operation of the equipment in the testing procedure. When regular control measurements show that the tolerances are not met, the equipment shall be rejected, adjusted or repaired. Records of control measurements shall be kept. Acceptance measurements on new equipment shall cover mass, volume, and dimensions to the extent that these are indicated in this document paying particular attention to those critical dimensions for which tolerances are specified.
In those cases where the material of the equipment can influence the results, the material is specified and shall be used.
oSIST prEN 196-1:2026 prEN 196-1 (E) The approximate dimensions shown in the figures are provided as guidance to equipment manufacturers or operators. Dimensions, which include tolerances, are obligatory.
5.3 Test sieves
Wire cloth test sieves conforming to ISO 3310-1 shall be of the sizes from ISO 565 given in Table 1 (series R 20).
Table 1 — Aperture of test sieves Square mesh size (mm) 2,00 1,60 1,00 0,50 0,16 0,08
5.4 Mixer
The mixer shall consist essentially of:
1) a stainless steel bowl with a capacity of about 5 l of the typical shape and size shown in Figure 1, provided with means by which it can be fixed securely to the mixer frame during mixing and by which the height of the bowl in relation to the blade and, to some extent, the gap between blade and bowl can be finely adjusted and fixed; 2) a stainless steel blade of the typical shape, size and tolerances shown in Figure 1, revolving about its own axis as it is driven in a planetary movement around the axis of the bowl at controlled speeds by an electric motor. The two directions of rotation shall be opposite and the ratio between the two speeds shall not be a whole number.
Blades and bowls shall form sets which shall always be used together. The gap of (3 ± 1) mm refers to the situation when the blade in the empty bowl shown in Figure 1 is brought as close as possible to the wall. This gap shall be checked regularly applying minimal pressure to the blade and assuring that there is no perceptible clearance between the joint of the blade and the axis of the motor.
NOTE 1 Simple tolerance gauges (feeler gauges) are useful where direct measurement is difficult. NOTE 2 The dimensions marked as approximate on Figure 1 are for the guidance of manufacturers. The mixer shall operate at the speeds given in Table 2 when mixing the mortar. Table 2 — Speeds of mixer blade Rotation around its own axis Planetary movement -1 –1 min min Low speed 140 ± 5 62 ± 5 High speed 285 ± 10 125 ± 10
oSIST prEN 196-1:2026 prEN 196-1 (E)
Key 1 bowl 2 blade Figure 1 — Typical bowl and blade
5.5 Moulds
The mould shall consist of three horizontal compartments so that three prismatic specimens 40 mm × 40 mm in cross section and 160 mm in length can be prepared simultaneously. A typical design is shown in Figure 2.
The mould shall be made of steel with walls approximately 10 mm thick. Each internal side face of the mould shall be case hardened to a Vickers hardness of at least HV 200, as supplied.
oSIST prEN 196-1:2026 prEN 196-1 (E) A minimum Vickers hardness value of HV 400 is recommended.
The mould shall be constructed in such a manner as to facilitate the removal of moulded specimens without damage. Each mould shall be provided with a machined steel or cast iron baseplate. The mould, when assembled, shall be positively and rigidly held together and fixed to the baseplate. The assembly shall be such that there is no distortion or visible leakage during operation. The baseplate shall make adequate contact with the table of the compacting apparatus and be rigid enough not to induce secondary vibrations.
NOTE 1 Moulds and jolting apparatus from different manufacturers can have unrelated external dimensions and masses, so their compatibility needs to be ensured by the purchaser. Each part of the mould shall be stamped with identifying marks to facilitate assembly and to ensure conformity to the specified tolerances. Similar parts of separate mould assemblies shall not be interchanged.
The assembled mould shall conform to the following requirements. a) The internal dimensions and tolerances of each mould compartment shall be as follows:
length: (160 ± 1) mm; width: (40,0 ± 0,2) mm; depth: (40,1 ± 0,1) mm.
b) The flatness tolerance (see ISO 1101) over the whole of each internal side face shall be not greater than 0,03 mm.
c) The perpendicularity tolerance (see ISO 1101) for each internal face with respect to the bottom surface of the mould and the adjacent internal face as datum faces shall be not greater than 0,2 mm.
d) The surface texture (see EN ISO 1302) of each internal side face shall be not rougher than N8, as supplied.
Moulds shall be replaced when any one of the specified tolerances is exceeded. The mass of the mould shall accord with the requirement for the combined mass in 5.6. In preparing the cleaned mould ready for use, a suitable sealing material shall be used to coat the outer joints of the mould. A thin film of mould oil shall be applied to the internal faces of the mould. NOTE 2 Some oils have been found to affect the setting of cement; mineral-based oils have been found to be suitable.
To facilitate the filling of the mould a tightly fitting metal hopper with vertical walls 20 mm to 40 mm in height shall be provided. When viewed in plan, the hopper walls shall overlap the internal walls of the mould by not more than 1 mm. The outer walls of the hopper shall be provided with a means of location to ensure correct positioning over the mould.
For spreading and striking off the mortar two spreaders and a metal straight-edge of the type shown in Figure 3 shall be provided.
oSIST prEN 196-1:2026 prEN 196-1 (E)
Key 1 striking off direction with sawing motion Figure 2 — Typical mould
oSIST prEN 196-1:2026 prEN 196-1 (E)
a) Large spreader
oSIST prEN 196-1:2026 prEN 196-1 (E)
b) Small spreader
oSIST prEN 196-1:2026 prEN 196-1 (E)
c) Straight-edge
Key D height of hopper Figure 3 — Typical spreaders and metal straight-edge
5.6 Jolting apparatus
The jolting apparatus (a typical design is shown in Figure 4) shall conform to the following requirements.
The apparatus shall consist of a rectangular table rigidly connected by two light arms to a pivot at nominally 800 mm from the centre of the table. The table shall incorporate at the centre of its lower face a projecting lug with a rounded face. Beneath the projecting lug shall be a small stop with a plane upper surface. In the rest position, the common normal through the point of contact of the lug and the stop shall be vertical. When the lug rests on the stop, the top face of the table shall be horizontal so that the level of any of the four corners does not deviate from the mean level by more than 1,0 mm. The table shall have dimensions equal to or greater than those of the mould baseplate, and a plane machined upper surface. Clamps shall be provided for firm attachment of the mould to the table. The combined mass of the table, including arms, empty mould, hopper and clamps shall be (20,0 ± 0,5) kg.
The arms connecting the table assembly to the pivot shall be rigid and constructed of round tubing with an outside diameter lying in the range 17 mm to 22 mm selected from tube sizes given in ISO 4200. The total mass of the two arms, including any cross bracing, shall be (2,25 ± 0,25) kg. The pivot bearings shall be of the ball or roller type and protected from ingress of grit or dust. The horizontal displacement of the centre of the table as caused by the play of the pivot shall not exceed 1,0 mm. The lug and the stop shall be made of through-hardened steel of at least HV 500 Vickers hardness value.
The curvature of the lug shall be about 0,01 mm .
In operation, the table is raised by a cam and allowed to fall freely from a height of (15,0 ± 0,3) mm before the lug strikes the stop.
The cam shall be made of through hardened steel of at least HV 400 Vickers hardness value and its shaft shall be mounted in ball bearings of such construction that the free fall is always (15,0 ± 0,3) mm. The cam follower shall be of a construction which ensures minimal wear of the cam. The cam shall be driven by an electric motor of about 250 W through a reduction gear at a uniform speed of one revolution per second. A control mechanism and a counter shall be provided which ensures that one period of jolting of (60 ± 3) s comprises exactly 60 jolts.
oSIST prEN 196-1:2026 prEN 196-1 (E) The position of the mould on the table shall be such that the longitudinal dimension of the compartments is in line with the direction of the arms and perpendicular to the axis of rotation of the cam. Suitable reference marks shall be provided to facilitate the positioning of the mould in such a way that the centre of the central compartment is directly above the point of impact. The apparatus shall be firmly mounted on a concrete block of mass of about 600 kg and volume of about
0,25 m and of dimensions giving a suitable working height for the mould. The entire base of the concrete block shall stand on an elastic pad, e.g. natural rubber, having a suitable isolation efficiency preventing external vibrations from affecting the compaction.
The base of the apparatus shall be fixed level to the concrete base by anchor bolts and a thin layer of mortar shall be placed between the base of the apparatus and the concrete base to ensure overall and vibration free contact.
The base of the apparatus shall be fixed level to the concrete base by anchor bolts to ensure overall and vibration free contact.
Key 1 lug 2 cam follower 3 cam 4 stop Figure 4 — Typical jolting apparatus
oSIST prEN 196-1:2026 prEN 196-1 (E)
5.7 Flexural strength testing apparatus
NOTE The provision of this apparatus is optional. If only the compressive strength is to be measured, prisms can be broken using other suitable means which do not subject the prism halves to harmful stresses. The flexural strength can be measured by using a flexural strength testing machine or by using a suitable device in a compression testing machine. In either case, the apparatus shall conform to the following requirements:
The apparatus for the determination of flexural strength shall be capable of applying loads up to 10 kN with an accuracy of ± 1,0 % of the recorded load in the upper four-fifths of the range being used, at a rate of loading of (50 ± 10) N/s.
The apparatus shall be provided with a flexure device incorporating two steel supporting rollers of (10,0 ± 0,5) mm diameter spaced (100,0 ± 0,5) mm apart and a third steel loading roller of the same diameter placed centrally between the other two. The length of these rollers shall be between 45 mm and 50 mm. The loading arrangement is shown in Figure 5.
a) Front view
b) Side view
Figure 5 — Arrangement of loading for determination of flexural strength The three vertical planes through the axes of the three rollers shall be parallel and remain parallel, equidistant and normal to the direction of the specimen under test. One of the supporting rollers and the loading roller shall be capable of tilting slightly to allow a uniform distribution of the load over the width of the specimen without subjecting it to any torsional stresses.
5.8 Compressive strength testing machine
The testing machine for the determination of compressive strength shall be of suitable capacity for the test (see Note 1): it shall have an accuracy of ± 1,0 % of the recorded load in the upper four-fifths of the range being used when verified in accordance with EN ISO 7500-1. It shall provide a rate of load increase of (2 400 ± 200) N/s. It shall be fitted with an indicating device which shall be so constructed that the value indicated at failure of the specimen remains indicated after the testing machine is unloaded. This can be achieved by the use of a maximum indicator on a pressure gauge or a memory on a digital display.
oSIST prEN 196-1:2026 prEN 196-1 (E) Manually operated testing machines shall be fitted with a pacing device to facilitate the control of the load increase.
...