Abstract

This International Standard specifies a method to determine the resistance to slow crack growth
(SCG) of polyethylene materials, pipes, and fittings. The test is applicable to samples taken from
compression moulded sheet or extruded pipes and injection moulded fittings of suitable thickness.
This International Standard provides a method that is suitable for an accelerated fracture-mechanics
characterization at ambient temperatures of 23 °C of different polyethylene grades, especially for PE
80 and PE 100 types for pipe applications.

Status
Not Published
Public Enquiry End Date
30-Dec-2025
Current Stage
5020 - Formal vote (FV) (Adopted Project)
Start Date
19-Oct-2026
Due Date
07-Dec-2026
Completion Date
19-Oct-2026

Buy Documents

Draft

oSIST prEN ISO 18489:2025 - BARVE

English language (24 pages)
Preview
Preview
e-Library read for
×1 day

kSIST FprEN ISO 18489:2026 is the SIST draft adoption of ISO 18489 for thermoplastic materials for piping systems. It specifies the Cracked Round Bar (CRB) test method used to determine resistance to slow crack growth (SCG) under cyclic loading, mainly for polyethylene (PE) materials, pipes and fittings. The method is aimed at laboratories and product teams that need a comparative fracture-mechanics test at 23 °C.

What does kSIST FprEN ISO 18489:2026 specify?

kSIST FprEN ISO 18489:2026 specifies how to run a cyclic tensile CRB test on cylindrical specimens with a circumferential notch, and how to turn the result into a slow crack growth ranking. The document is organised so that the general method comes first, followed by material-specific annexes for PE, PP and PA-U.

The scope covers samples taken from compression moulded sheets, extruded rods or pipes, and injection moulded fittings of suitable thickness. It also states that the method can be used for virgin and non-virgin thermoplastic materials, and that it can be adapted to other thermoplastics by developing suitable test parameters.

AnnexWhat it covers
Annex ARecalculation between different test specimen diameters and single point interpolation
Annex BTest parameters for PE
Annex CTest parameters for PP
Annex DTest parameters for PA-U (PA-U11, PA-U12)

What are the key requirements of kSIST FprEN ISO 18489:2026?

kSIST FprEN ISO 18489:2026 is built around a controlled cyclic load test, careful specimen preparation, and post-test evaluation of fracture surfaces. In practice, the standard matters because the result is only meaningful if the notch geometry, loading, conditioning and data reduction are all kept within the stated limits.

Test principle and loading

Clause 4 states that the specimen is loaded in tension with a constant load range until final failure, while a circumferential notch promotes crack initiation and slow crack growth. The number of cycles to failure is then related to the applied stress range and the initial crack length. For a reader, this means the test is not a simple strength check - it is designed to compare how materials resist crack growth over time.

Clause 5 requires a machine that can apply and record a cyclic load with a sinusoidal waveform, with maximum and minimum load held constant in load control mode within ±1%. The frequency must also be controlled within ±1%. This matters because drift in load or frequency changes the crack-growth rate and can make results difficult to compare.

Specimen geometry, preparation and conditioning

Clause 6 defines the CRB specimen as a cylindrical bar with a notch in the middle. The nominal dimensions are tightly controlled, including the specimen length, diameter, target initial crack length and the minimum distance from the notch to the grips. That prevents clamping effects from influencing the crack tip.

The same clause requires machining in accordance with ISO 2818, notching at ambient 23 °C, and care to avoid heating, blunting or residual stress at the notch. The notching guidance is practical: the notch must be razor sharp, perpendicular to the axis, and made with a blade that is not worn out. After notching, specimens are conditioned at 23/50, Class 2 according to ISO 291 for at least 24 h unless otherwise specified.

Test procedure and evaluation

Clause 7 requires the specimen diameter to be measured on both sides of the notch before testing, without measuring directly in the notch. It also requires careful mounting so that the specimen is not bent, twisted or preloaded. For the reader, this means the set-up must preserve a pure axial test condition.

The load ratio is fixed at R = 0,1, and the test is run at different target stress ranges. At least four specimens are required, each at a different stress level, and the stress levels should span the relevant range for the material. The load is applied continuously until failure, and static loading before the cyclic test is avoided.

Clause 7.7 explains how the initial crack length is determined after the test from the fracture surface, using the measured initial ligament diameter and microscope-based evaluation. That post-test measurement is important because the true crack size at the start of the test cannot be read accurately from the unloaded notch alone.

Data treatment, validity and reporting

Clause 8 requires only failures in the plane of the razor notch to be used. The applied stress range is corrected using the measured fracture-surface dimensions, and the results are plotted in a double logarithmic diagram of stress range versus failure cycle number. A linear regression is then used to fit the data, and the coefficient of determination is checked. If the fit is too weak, additional testing is required, and the test becomes invalid if the required fit quality is not reached.

Clause 9 lists what the test report has to capture: material identification, specimen preparation, notching details, measured dimensions, test equipment, atmosphere, loading variables, the graph of stress range versus cycles, fracture-surface photographs, laboratory name and any factors that could have affected the result. In practice, this makes the report usable for ranking materials, audits and later review.

Annexes for comparison and material-specific settings

Annex A is important when specimens have different diameters. It explains how results can be compared through the stress intensity factor range, and it also gives a single-point interpolation approach based on reference geometry. Annexes B, C and D provide the material-specific moulding conditions, loading frequencies and typical stress ranges for PE, PP and PA-U.

What terms does kSIST FprEN ISO 18489:2026 define?

kSIST FprEN ISO 18489:2026 defines the main quantities used to describe the CRB test and its results.

  • Cycle - the repeating load-time or stress-time segment used in the cyclic test.
  • Failure cycle number - the total number of cycles from the start of the test until specimen failure.
  • Frequency - the number of cycles per second, expressed in hertz (Hz).
  • Load ratio (R) - the ratio of minimum load to maximum load in one cycle.
  • Load range (ΔF) - the difference between maximum and minimum load in one cycle.
  • Initial crack length - the crack depth at the start of the test, calculated after testing.
  • Initial ligament diameter - the remaining cylindrical ligament after notching, measured after testing.
  • Stress range (Δσ) - the difference between maximum and minimum stress at the beginning of the test.

Who uses kSIST FprEN ISO 18489:2026?

kSIST FprEN ISO 18489:2026 is used by testing laboratories, pipe and fitting manufacturers, polymer compounders, and technical teams that need to compare slow crack growth resistance. It is especially relevant in the plastics piping industry, where long-term crack resistance affects pipes, fittings and related components.

The standard is also useful for quality managers and buyers who need a repeatable test method for material selection, incoming material control, product qualification or comparative ranking. Because it includes PE, PP and PA-U settings, it supports both development work and specification work for different thermoplastic piping materials.

What changed in kSIST FprEN ISO 18489:2026 from the previous edition?

kSIST FprEN ISO 18489:2026 replaces ISO 18489:2015, and the foreword says the document has been technically revised. The stated changes are:

  • Clause 7.7 was improved for the calculation of the initial crack length.
  • Annex A was improved for recalculation between different specimen diameters, with added information for single-point evaluation.
  • The material test parameters were moved into Annexes B, C and D, with PP and PA-U added.
  • New photographs of PE fracture surfaces after testing were included.

Which standards are used with kSIST FprEN ISO 18489:2026?

kSIST FprEN ISO 18489:2026 names several standards that support specimen preparation, conditioning and material-specific use.

  • ISO 291 - provides the standard atmospheres used for conditioning and testing.
  • ISO 2818 - gives the machining rules for preparing plastic test specimens.
  • ISO 16396-1 - supports designation and specification basis for PA materials.
  • ISO 16396-2 - supports PA specimen preparation and property determination.
  • ISO 16770 - is the basis for the PE compression moulding conditions used in Annex B.
  • CEN/TS 14541-2:2022 - is referenced in Annex C for PP recyclates.
  • EN 14758-1:2023 - is referenced in Annex C for PP-MD piping systems.
  • ISO 16486-1 - is referenced in Annex D for PA-U 11 180 and PA-U 12 180 pipe material context.

What does the kSIST FprEN ISO 18489:2026 document contain?

kSIST FprEN ISO 18489:2026 contains the full test method, from principle through reporting, plus material-specific annexes. It includes the apparatus requirements, specimen geometry, notching method, conditioning rules, loading calculations, data treatment and the required report content.

The document also includes figures showing the specimen configuration, load calculation, crack-length evaluation and an example stress-range versus failure-cycle graph. Formulae are provided for load calculation, stress correction after testing, and the Annex A recalculation and interpolation methods. Tables in the annexes give the moulding conditions, typical load frequencies and stress ranges used for PE, PP and PA-U, which makes the document usable both for routine testing and for setting up a test program.

Relations

Effective Date
28-Jan-2026
Effective Date
28-Jan-2026
Effective Date
28-Jan-2026
Effective Date
28-Jan-2026
Effective Date
28-Jan-2026
Effective Date
28-Jan-2026

Buy Documents

Draft

oSIST prEN ISO 18489:2025 - BARVE

English language (24 pages)
Preview
Preview
e-Library read for
×1 day

Get Certified

Connect with accredited certification bodies for this standard

Institut za varilstvo d.o.o. (Welding Institute)

Slovenia's leading welding institute since 1952. ISO 3834, EN 1090, pressure equipment certification, NDT personnel, welder qualification. Only IIW Au

SA Slovenia Verified

Sponsored listings

Frequently Asked Questions

kSIST FprEN ISO 18489:2026 is a draft published by the Slovenian Institute for Standardization (SIST). Its full title is "Thermoplastic materials for piping systems - Determination of resistance to slow crack growth under cyclic loading - Cracked Round Bar (CRB) test method (ISO/DIS 18489:2025)". This standard covers: This International Standard specifies a method to determine the resistance to slow crack growth (SCG) of polyethylene materials, pipes, and fittings. The test is applicable to samples taken from compression moulded sheet or extruded pipes and injection moulded fittings of suitable thickness. This International Standard provides a method that is suitable for an accelerated fracture-mechanics characterization at ambient temperatures of 23 °C of different polyethylene grades, especially for PE 80 and PE 100 types for pipe applications.

This International Standard specifies a method to determine the resistance to slow crack growth (SCG) of polyethylene materials, pipes, and fittings. The test is applicable to samples taken from compression moulded sheet or extruded pipes and injection moulded fittings of suitable thickness. This International Standard provides a method that is suitable for an accelerated fracture-mechanics characterization at ambient temperatures of 23 °C of different polyethylene grades, especially for PE 80 and PE 100 types for pipe applications.

kSIST FprEN ISO 18489:2026 is classified under the following ICS (International Classification for Standards) categories: 23.040.45 - Plastics fittings. The ICS classification helps identify the subject area and facilitates finding related standards.

kSIST FprEN ISO 18489:2026 has the following relationships with other standards: It is inter standard links to SIST EN ISO 19403-3:2025, SIST EN ISO 19403-5:2025, SIST EN ISO 19403-2:2025, SIST EN ISO 19403-4:2025, SIST EN ISO 19403-6:2025, SIST EN ISO 19403-7:2025. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.

kSIST FprEN ISO 18489:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)

Contents

  • Introduction
  • 1 Scope
  • 2 Normative references
  • 3 Terms and definitions
  • 3.1 cycle
  • 3.2 failure cycle number
  • 3.3 frequency
  • 3.4 initial crack length
  • 3.5 initial ligament diameter
  • 3.6 load ratio
  • 3.7 load range
  • 3.8 maximum load
  • 3.9 minimum load
  • 3.10 notch distance
  • 3.11 target initial crack length
  • 3.12 target initial ligament diameter
  • 3.13 target stress range
  • 3.14 specimen diameter
  • 3.15 specimen length
  • 3.16 stress range
  • 3.17 waveform
  • 3.18 reference specimen radius
  • 3.19 reference specimen diameter
  • 3.20 reference initial crack length
  • 3.21 reference stress range
  • 3.22 reference stress intensity factor
  • 4 Principle
  • 5 Apparatus
  • 5.1 Test machine
  • 5.2 Microscope
  • 5.3 Notching apparatus
  • 6 Test specimen
  • 6.1 Specimen geometry and dimensions
  • 6.2 Test specimen preparation
  • 6.3 Specimen notching
  • 6.4 Specimen conditioning
  • 7 Test procedure
  • 7.1 Measurement of specimen dimensions
  • 7.2 Specimen mounting
  • 7.3 Test atmosphere
  • 7.4 Calculation of test load
  • 7.5 Load-cycle frequency
  • 7.6 Load application
  • 7.7 Initial crack length calculation
  • 8 Data treatment
  • 9 Test report
  • Annex A
  • Annex B
  • Annex C
  • Annex D
  • Bibliography

Introduction

Knowledge about the resistance to long-term failure mechanisms as a result of crack initiation and slow crack growth (SCG) is important for the ranking and pre-selection of thermoplastic materials, especially for long-term applications such as pipes and fittings made of thermoplastic pipe materials. Several tests to determine the relevant failure mechanisms are available today where elevated temperatures and also the combination with stress cracking liquids are used to decrease the time frame for testing. Developments in modern polyethylene materials have led to a significant increase of resistance to crack initiation and slow crack growth so that testing with available methods exceeds practical time frames. Therefore, new accelerated methods, preferably at application relevant temperatures and without additional time reducing liquids, are required.

This test method achieves a significant decrease of testing time even at ambient temperatures of 23 °C. This is more relevant to the temperature range of many applications and testing at this temperature does not change the structural status of the polymer. Acceleration of material testing is achieved by the specimen [2] [3] [4] geometry and the cyclic loading regime to result in completion of testing in a relatively short time , , .

oSIST prEN ISO 18489:2025

oSIST prEN ISO 18489:2025 DRAFT International Standard ISO/DIS 18489:2025(en) Thermoplastic materials for piping systems — Determination of resistance to slow crack growth under cyclic loading — Cracked Round Bar (CRB) test method

1 Scope

This document specifies a method to determine the resistance to slow crack growth (SCG) of thermoplastic materials, pipes, and fittings. The test is applicable to samples taken from compression moulded sheets, extruded rods, sheets or pipes and injection moulded fittings of suitable thickness. This document provides a method that is suitable for an accelerated fracture-mechanics characterization at ambient temperatures of 23 °C.

This document specifies test parameters for polyethylene (PE), polypropylene (PP) and unplasticized polyamide (PA-U).

Furthermore, this test can be applied to characterise the slow crack growth resistance of virgin, as well as [5] non-virgin (reused, recycled) thermoplastic materials.

This test method can be adapted for other thermoplastics materials by developing the procedure using different test parameters.

2 Normative references

The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 291, Plastics — Standard atmospheres for conditioning and testing ISO 2818, Plastics — Preparation of test specimens by machining ISO 16396-1, Plastics — Polyamide (PA) moulding and extrusion materials — Part 1: Designation system and basis for specifications ISO 16396-2, Plastics — Polyamide (PA) moulding and extrusion materials — Part 2: Preparation of test specimens and determination of properties ISO 16770, Plastics — Determination of environmental stress cracking (ESC) of polyethylene — Full-notch creep test (FNCT) CEN/TS 14541-2:2022, Plastics pipes and fittings — Utilisation of thermoplastics recyclates — Part 2:

Recommendations for relevant characteristics EN 14758-1:2023, Plastics piping systems for non-pressure underground drainage and sewerage — Polypropylene with mineral modifiers (PP-MD) — Part 1: Specifications for pipes, fittings and the system

3 Terms and definitions

For the purposes of this document, the following terms and definitions apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:

  • ISO Online browsing platform: available at https:// www .iso .org/ obp

oSIST prEN ISO 18489:2025 ISO/DIS 18489:2025(en) - IEC Electropedia: available at https:// www .electropedia .org/

3.1 cycle

N smallest segment of a load-time or stress-time function which is repeated periodically

3.2 failure cycle number

N f total number of cycles (3.1) from the beginning until failure of the test specimen

3.3 frequency

f number of cycles (3.1) within one second Note 1 to entry: It is expressed in hertz (Hz).

3.4 initial crack length

a ini depth of the crack from the specimen surface through the crack tip at the beginning of the test, calculated after testing Note 1 to entry: It is expressed in millimetres (mm).

3.5 initial ligament diameter

D ini ligament diameter of the cylindrical specimen after notching at the beginning of the test, measured after testing Note 1 to entry: It is expressed in millimetres (mm).

3.6 load ratio

R ratio of the minimum load F (3.19) to the maximum load F (3.8) in one cycle (3.1) min max Note 1 to entry: It is calculated by F min R= F max

3.7 load range

ΔF difference between the maximum load F (3.8) and minimum load F (3.9) in one cycle (3.1) max min Note 1 to entry: It is expressed in Newtons (N).

3.8 maximum load

F max highest value of the applied load, in Newtons (N), in one cycle (3.1)

3.9 minimum load

F min lowest value of the applied load, in Newtons (N), in one cycle (3.1)

oSIST prEN ISO 18489:2025 ISO/DIS 18489:2025(en)

3.10 notch distance

L min minimum distance from notch to clamping system Note 1 to entry: It is expressed in millimetres (mm).

3.11 target initial crack length

a * ini target depth of the crack from the specimen surface through the crack tip after notching, prior to testing Note 1 to entry: It is expressed in millimetres (mm).

3.12 target initial ligament diameter

D * ini target ligament diameter of the cylindrical specimen after notching, prior to testing Note 1 to entry: It is expressed in millimetres (mm).

Note 2 to entry: It is calculated by D * = D – 2 a * ini ini

3.13 target stress range

Δσ *

target difference between the maximum and minimum stress at the beginning of the test Note 1 to entry: It is expressed in megapascals (MPa).

3.14 specimen diameter

D diameter of the cylindrical specimen measured prior to testing, measured after notching at the vicinity of notch location Note 1 to entry: It is expressed in millimetres (mm).

3.15 specimen length

L total length of the test specimen Note 1 to entry: It is expressed in millimetres (mm).

3.16 stress range

Δσ

applied difference between the maximum and minimum stress at the beginning of the test Note 1 to entry: It is expressed in megapascals (MPa).

3.17 waveform

shape of the load-time curve within a single cycle (3.1)

3.18 reference specimen radius

r ref reference specimen radius (D = 2r ), given in the product standard or requirement, used for recalculation ref ref after testing using Annex A Note 1 to entry: It is expressed in millimetres (mm).

oSIST prEN ISO 18489:2025 ISO/DIS 18489:2025(en)

3.19 reference specimen diameter

D ref reference specimen diameter (D = 2r ), given in the product standard or requirement, used for ref ref recalculation after testing using Annex A Note 1 to entry: It is expressed in millimetres (mm).

3.20 reference initial crack length

a ini-ref reference depth of the crack, given in the product standard or requirement, used for recalculation after testing using Annex A Note 1 to entry: It is expressed in millimetres (mm).

3.21 reference stress range

Δσ 0-ref difference between the maximum and minimum stress calculated using equation A.3 based on a reference specimen diameter and reference initial crack length Note 1 to entry: It is expressed in megapascals (MPa).

3.22 reference stress intensity factor

ΔK I-ref difference between minimum and maximum stress intensity factor calculated using equation A.1 based on a reference specimen diameter and reference initial crack length 0,5 Note 1 to entry: It is expressed in megapascals per square root metre (MPa m ).

4 Principle

A cyclic tensile test with constant load range is imposed on a cylindrical specimen under suitable test conditions within the stress range where SCG is achieved. A circumferential notch is machined in the centre of the test specimen to enable crack initiation and SCG to final failure of the specimen. The number of cycles until final failure, N , is recorded as a function of the stress range, Δσ , at the initial crack length, a . The f 0 ini specimen geometry ensures quick crack initiation and short testing times due to the high constraint and low plastics deformations along the crack tip.

5 Apparatus

5.1 Test machine

5.1.1 Loading system

The loading system shall be capable of imposing and recording a cyclic load. The cyclic load shall follow a sinusoidal waveform which is characterized by the maximum load, F , and max the load ratio, R. The maximum and minimum loading values shall be constant (load control mode) during the entire test with an accuracy of ±1 %.

The load-cycle frequency shall have an accuracy of ±1 %.

5.1.2 Grips

The grips shall be suitable to clamp cylindrical specimens. It shall ensure that the load distribution is in alignment with the specimen axis.

oSIST prEN ISO 18489:2025 ISO/DIS 18489:2025(en)

5.1.3 Temperature chamber

For testing at low or high temperatures the test machine shall be equipped with a suitable chamber that contains the environment and ensures complete exposure of the specimen. The chamber shall be constructed of materials which do not affect the environment and which are not affected by it. The temperature of the environment shall be controlled in order to maintain the test specimens within ±2 °C of the specified temperature.

5.2 Microscope

A microscope with an accuracy of 0,03 mm or an equivalent device shall be used to determine the initial crack length after the finished cyclic tests.

5.3 Notching apparatus

The device used shall be capable of producing a razor-sharp notch of defined depth at the circumference of the cylindrical specimen. The notch tip radius produced shall be less than 10 μm. NOTE Usually, razor blades meet this requirement.

A conventional lathe in combination with a razor blade tool may be suitable for this purpose. Bending of the razor blade shall be avoided and notching perpendicular to the specimen axis shall be ensured. It is recommended to use a razor blade support where the free length of the razor blade for notching is limited to approximately 2 mm for notch depths of 1,4 mm.

6 Test specimen

6.1 Specimen geometry and dimensions

The specimen configuration of the cracked round bar (CRB) specimen is shown in Figure 1. A cylindrical bar of length, L, and diameter, D, is prepared with a circumferential razor-sharp notch with a depth of a * ini (target initial crack length) in the middle of the specimen resulting in a target initial ligament diameter, D *. ini Specimen dimensions shall be as specified in Table 1. The initial crack shall be perpendicular to the specimen axis.

To avoid clamping effects at the crack tip, the notch distance, L , shall be at least 20 mm from the grips. min Table 1 — Specimen dimensions dimension parameter mm L specimen length 80 to 100 D specimen diameter 14,0 ± 0,15 a * target initial crack length 1,40 ini minimum distance between L ≥20 min notch and clamping system Clamping part of the specimen may be threaded, for example, M 14 × 1,0 metric fine thread, in which case matching grips shall be used.

NOTE Alternative dimensions can be used, but results are to be compared by the stress intensity factor range instead of the stress range (see Annex A).

oSIST prEN ISO 18489:2025 ISO/DIS 18489:2025(en) Key L specimen length L minimum distance between notch and clamping system min a * target initial crack length ini D * target initial ligament diameter ini D specimen diameter 1 razor-sharp notch Figure 1 — Principal configuration of CRB test specimen with optional metric fine thread

6.2 Test specimen preparation

The test specimens shall be machined from compression moulded sheets, extruded rods or directly from pipe or fittings. The use of different processing conditions can affect the results. Conditions for compression moulding of test specimens are given in the Annexes for the individual materials. The specimens shall be machined in accordance with ISO 2818.

...