ISO/PRF 24819
(Main)Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding
- Abstract
The standardisation of the test methods used to characterise the compaction response of fibrous reinforcements used in the manufacture of composite materials by liquid composite moulding. The test method provides a measurement of the peak compression stress at a defined volume fraction on both dry and wet specimens, mirroring the conditions of liquid composite moulding processes
- Status
- Not Published
- Technical Committee
- ISO/TC 61/SC 13 - Composites and reinforcement fibres
- Drafting Committee
- ISO/TC 61/SC 13/WG 1 - Reinforcements and reinforcement products
- Current Stage
- 5020 - Proof sent to secretariat or FDIS ballot initiated: 8 weeks - 50 Approval
- Start Date
- 29-Oct-2026
Buy Documents
ISO/PRF 24819 - Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding
REDLINE ISO/PRF 24819 - Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding
ISO/PRF 24819 is an ISO standard for testing the compaction response of fibrous reinforcements used in liquid composite moulding (LCM). It specifies a laboratory method for measuring peak compaction pressure at a defined thickness or fibre volume fraction on dry and wet specimens, so users can compare reinforcement textiles under conditions that reflect composite manufacture.
What does ISO/PRF 24819 specify?
ISO/PRF 24819 specifies a test method for characterising the compaction response of fibrous reinforcements used in liquid composite moulding. The document is organized into clauses on the principle, design of experiments, specimen preparation, test procedure, data analysis, precision, and reporting, with two informative annexes.
| Annex | What it covers |
|---|---|
| Annex A | Precision data from interlaboratory comparison exercises |
| Annex B | Compliance measurement for correcting crosshead displacement |
The method applies to fibrous reinforcement textiles in dry form and in a saturated state. In practice, that means the same type of material can be checked both as received and under a wet condition that mimics resin saturation during manufacture.
What are the key requirements of ISO/PRF 24819?
ISO/PRF 24819 requires a controlled compression test, careful specimen preparation, and reporting of compaction pressure versus thickness. The main practical point is that small changes in setup, specimen handling, or speed can change the result, so the document gives detailed guidance to keep tests comparable.
Test principle and machine setup
ISO/PRF 24819 loads a specimen in compression at constant speed until a defined thickness is reached, then unloads it at the same speed. The load is recorded continuously and can be held at thickness for an optional relaxation period.
The test machine is a universal test machine (UTM) suitable for compression and in line with ISO 5893 as appropriate. The platens must be larger than the specimen, self-aligning, lockable in alignment, and flat and parallel within ±0.03 mm. This matters because platen misalignment can distort the measured compaction response.
Measurement and data acquisition
ISO/PRF 24819 calls for direct thickness measurement with a calibrated sensor such as an extensometer, laser displacement system, or linear variable differential transformer (LVDT). The displacement sensor accuracy shall be ±0.01 mm, and the load cell shall have a valid calibration certificate with load error not exceeding ±1 % of applied full load.
The document also allows compliance-corrected thickness from UTM crosshead displacement, with details in Annex B. In practice, that helps separate true specimen compression from machine and fixture deformation.
Specimen preparation
ISO/PRF 24819 requires fabrics to be conditioned in the laboratory environment for 24 h before measurement. Specimens are to be cut with high geometric accuracy, visually checked for defects, and measured accurately for size.
For stacked specimens, the reference direction and reference side must be defined, and layers aligned consistently unless another layup is specified. The stack should normally have 10 to 20 layers, or at least 3 mm height for materials that cannot be layered in the usual way. Each specimen must have a unique identifier, which supports traceability and repeat testing.
Wet tests and temperature
ISO/PRF 24819 allows wet testing with a quasi-Newtonian, incompressible fluid of viscosity between 70 mPa·s and 200 mPa·s at the test temperature. The specimen is immersed for 15 minutes and then drained horizontally for 15 minutes.
The test shall be performed under isothermal conditions. This matters because compaction behavior can vary with temperature and fluid condition, especially when the wet test is used to mimic saturation during LCM.
Repeats, analysis, and reporting
ISO/PRF 24819 states that compaction tests are destructive, so repeat tests must use new specimens. At least five repeats are required for each test condition, unless the work is specifically studying quasi-viscoelastic effects with repeated cycles on the same specimen.
The data analysis calculates compaction pressure from load and contact area, then fits a power-law relation between thickness and compaction pressure separately for loading and unloading curves. The document recommends an R value of at least 0.95 for the fit. The test report must include specimen identity, preparation, dimensions, test conditions, number of specimens, individual measurements, mean values for the fit constants and R coefficient, standard deviations if needed, and the peak compaction pressure.
What terms does ISO/PRF 24819 define?
- Compaction pressure - the compressive force carried by the specimen divided by its initial cross-sectional area.
- Peak compaction pressure - the maximum value of the compressive load reached during the test.
- Thickness - the distance between the top and bottom compression platens when they are in contact with the specimen.
- Area - the contact area between the specimen and the compression platens.
- Compliance measurement - the total system deformation per unit of force, used to correct crosshead displacement.
- Fibre volume fraction - the fraction of the specimen volume occupied by fibre, derived from fabric thickness, areal weight, number of layers, and fibre density.
Who uses ISO/PRF 24819?
ISO/PRF 24819 is used by laboratories, composite manufacturers, material suppliers, and quality teams working with reinforcement textiles for polymer matrix composites. It supports material development, incoming material checks, process development for liquid composite moulding, and comparison of dry and wet reinforcement behavior. Buyers and technical reviewers can also use it to specify how compaction data should be generated and reported.
Which standards are used with ISO/PRF 24819?
ISO 5893 is the main referenced standard. It supports the requirements for the compression-type test machine used in the method.
ISO 5725-2 is used in Annex A for the treatment of repeatability and reproducibility data from the interlaboratory comparison work.
What does the ISO/PRF 24819 document contain?
ISO/PRF 24819 contains the test principle, equipment and fixture requirements, specimen preparation steps, wet specimen conditioning, the test sequence, and the calculations used to turn force-displacement data into compaction pressure. It also includes a figure showing the wetting and draining setup for saturated specimens.
Annex A presents precision data from interlaboratory comparison exercises, including repeatability and reproducibility results. Annex B gives the compliance measurement method used to support corrected thickness measurement from UTM crosshead displacement.
Buy Documents
ISO/PRF 24819 - Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding
REDLINE ISO/PRF 24819 - Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding
Get Certified
Connect with accredited certification bodies for this standard
DIN CERTCO
DIN Group product certification.

Smithers Quality Assessments
US management systems and product certification.
Sponsored listings
Frequently Asked Questions
ISO/PRF 24819 is a draft published by the International Organization for Standardization (ISO). Its full title is "Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding". This standard covers: The standardisation of the test methods used to characterise the compaction response of fibrous reinforcements used in the manufacture of composite materials by liquid composite moulding. The test method provides a measurement of the peak compression stress at a defined volume fraction on both dry and wet specimens, mirroring the conditions of liquid composite moulding processes
The standardisation of the test methods used to characterise the compaction response of fibrous reinforcements used in the manufacture of composite materials by liquid composite moulding. The test method provides a measurement of the peak compression stress at a defined volume fraction on both dry and wet specimens, mirroring the conditions of liquid composite moulding processes
ISO/PRF 24819 is classified under the following ICS (International Classification for Standards) categories: 83.120 - Reinforced plastics. The ICS classification helps identify the subject area and facilitates finding related standards.
ISO/PRF 24819 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 3.1 compaction pressure
- 3.2 peak compaction pressure
- 3.3 thickness
- 3.4 area
- 3.5 compliance measurement
- 4 Principle
- 5 Design of experiments
- 5.1 Test machine and loading fixtures
- 5.2 Data acquisition
- 5.3 Temperature conditions
- 5.4 Calculation of the fibre volume fraction
- 5.5 Selecting the crosshead speed and hold time
- 5.6 Number of repeat tests
- 6 Test specimen and specimen preparation
- 6.1 Fabric storage
- 6.2 Fabric conditioning
- 6.3 Specimen cutting
- 6.4 Specimen stacking
- 6.5 Specimen mass measurement
- 6.6 Specimen preparation for wet tests
- 7 Test procedure
- 8 Data analysis
- 9 Precision
- 10 Test report
- Annex A
- Annex B
- Bibliography
Introduction
This document presents a standard for the characterisation of reinforcement textiles under compression by measuring the compressive load at a given thickness, for the purposes of understanding the behaviour of such materials during the composites manufacturing process. This document has been developed following two interlaboratory trials used to establish a practical and repeatable test method. The method presented here aims to minimize errors by providing guidance on specimen preparation and test setup, to which the results can be highly sensitive. This document can be applied to any fibrous reinforcement textile to be used in the manufacture of a polymer matrix composite. Tests can be carried out on wet or dry specimens, where the wet specimen condition is used to mimic saturation during manufacture. PROOF/ÉPREUVE
International Standard ISO 24819:2026(en) Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding
1 Scope
This document specifies the method for the characterisation of the compaction response of fibrous reinforcements used in liquid composite moulding.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 5893, Rubber and plastics test equipment — Tensile, flexural and compression types (constant rate of traverse) — Specification
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- ISO Online browsing platform: available at https:// www .iso .org/ obp
- IEC Electropedia: available at https:// www .electropedia .org/
3.1 compaction pressure
compressive force, carried by the test specimen at any particular moment, divided by the initial crosssectional area of the specimen
3.2 peak compaction pressure
maximum value of the compressive load
3.3 thickness
distance between the top and bottom compression platens, if in contact with the tested specimen
3.4 area
contact area between the specimen and the compression platens
3.5 compliance measurement
total system deformation per unit of force Note 1 to entry: Measured in mm per N.
PROOF/ÉPREUVE
ISO 24819:2026(en)
4 Principle
Test specimens are loaded in compression at a constant speed until a defined thickness is reached. The compressive load is measured. In some tests, the compression may be held for a fixed period of time. The specimen is then unloaded at a constant speed. The peak compaction pressure exerted is calculated from the measured force-displacement curve.
Tests can be carried out on specimens in both the unsaturated (“dry”) and saturated (“wet”) state. For specimen saturation, a model fluid is used, such as silicone oil, that mimics resin-saturated reinforcements during liquid composite moulding (LCM).
This method specifies the speed of testing. It should be noted that testing at different speeds can yield different results which might not be comparable.
5 Design of experiments
5.1 Test machine and loading fixtures
This test shall be carried out using a universal test machine (UTM) which can be used in compression. The test machine shall be in accordance with ISO 5893 as appropriate. The testing machine shall be capable of maintaining the required speed of testing.
The platens shall be square or round and shall be larger than the specimen area. Self-aligning platens shall be used in this test. They shall be lockable in the aligned position and remain locked during compression. The contact surfaces shall be flat and parallel to within ±0,03 mm, which should be measured using a dial indicator.
Pressure paper can be used as a qualitative parallelism check by placing a sheet of pressure paper between the platens and compressing to a recommended load of 10 kN and checking that the colour change across the paper is even across the contact area of the platen.
5.2 Data acquisition
Thickness measurements shall be obtained with a calibrated sensor capable of direct measurement of the distance between the compression platens. Examples include:
- extensometer;
- laser displacement measurement;
- linear variable differential transformer (LVDT).
The accuracy of the displacement sensor shall be ±0,01 mm.
The thickness measurements obtained via direct sensing methods can be supplemented by compliancecorrected thickness measurements taken from the crosshead displacement of the UTM. Details of this method are provided in Annex B.
Load measurements are to be taken from the load cell of the UTM. The load cell shall have a valid calibration certificate. The error for the indicated load shall not exceed ±1 % of applied full load.
5.3 Temperature conditions
The test shall be performed under isothermal conditions.
PROOF/ÉPREUVE
ISO 24819:2026(en)
5.4 Calculation of the fibre volume fraction
The thickness used in the test is equivalent to the displacement between platens. This can be related to the fibre volume fraction using Formula (1):
An w V (1) f t where t is the thickness of the fabric; A is the areal weight of the fabric; w n is the number of layers of fabric in the specimen; ρ is the density of a fibre the fabric; V is the fibre volume fraction.
...
Contents
- Introduction
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 3.5 compliance measurement
- 4 Principle
- 5 Design of experiments
- 5.1 Test machine and loading fixtures
- 5.2 Data acquisition
- 5.3 Temperature conditions
- 5.4 Calculation of the fibre volume fraction
- 5.5 Selecting the crosshead speed and hold time
- 5.6 Number of repeat tests
- 6 Test specimen and specimen preparation
- 6.1 Fabric storage
- 6.2 Fabric conditioning
- 6.3 Specimen cutting
- 6.4 Specimen stacking
- 6.5 Specimen mass measurement
- 6.6 Specimen preparation for wet tests
- 7 Test procedure
- 8 Data analysis
- 9 Precision
- 10 Results documentation
- 10 Test report
- Annex A
- Annex B
- Bibliography
Introduction
This document presents a standard for the characterisation of reinforcement textiles under compression by measuring the compressive load at a given thickness, for the purposes of understanding the behaviour of such materials during the composites manufacturing process. This document has been developed following two interlaboratory trials used to establish a practical and repeatable test method. The method presented here aims to minimiseminimize errors by providing guidance on specimen preparation and test setup, to which the results can be highly sensitive. This document can be applied to any fibrous reinforcement textile to be used in the manufacture of a polymer matrix composite. Tests can be carried out on wet or dry specimens, where the wet specimen condition is used to mimic saturation during manufacture.
ISO/PRF 24819:2026(en) Plastics — Experimental characterisation of the compaction response of fibrous reinforcements for liquid composite moulding
1 Scope
This document specifies the method for the characterisation of the compaction response of fibrous reinforcements used in liquid composite moulding.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. ISO 5893, Rubber and plastics test equipment — Tensile, flexural and compression types (constant rate of traverse) — Specification
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- — ISO Online browsing platform: available at https://www.iso.org/obp
- — IEC Electropedia: available at https://www.electropedia.org/ 3.1 3.1 compaction pressure compressive force, carried by the test specimen at any particular moment, divided by the initial cross-sectional area of the specimen 3.2 3.2 peak compaction pressure maximum value of the compressive load 3.3 3.3 thickness distance between the top and bottom compression platens, if in contact with the tested specimen 3.4 3.4 area contact area between the specimen and the compression platens
3.5 compliance measurement
total system deformation per unit of force Note 1 to entry: Measured in mm per N.
4 Principle
Test specimens are loaded in compression at a constant speed until a defined thickness is reached. The compressive load is measured. In some tests, the compression may be held for a fixed period of time. The
ISO/PRF 24819:2026(en) specimen is then unloaded at a constant speed. The peak compaction pressure exerted is calculated from the measured force-displacement curve.
Tests can be carried out on specimens in both the unsaturated (“dry”) and saturated (“wet”) state. For specimen saturation, a model fluid is used, such as silicone oil, that mimics resin-saturated reinforcements during liquid composite moulding (LCM).
This method specifies the speed of testing. It should be noted that testing at different speeds can yield different results which might not be comparable.
5 Design of experiments
5.1 Test machine and loading fixtures
This test shall be carried out using a universal test machine (UTM) which can be used in compression. The test machine shall be in accordance with ISO 5893 as appropriate. The testing machine shall be capable of maintaining the required speed of testing.
The platens shall be square or round and shall be larger than the specimen area. Self-aligning platens shall be used in this test. They shall be lockable in the aligned position and remain locked during compression. The contact surfaces shall be flat and parallel to within ±0,03 mm, which should be measured using a dial indicator.
Pressure paper can be used as a qualitative parallelism check by placing a sheet of pressure paper between the platens and compressing to a recommended load of 10 kN and checking that the colour change across the paper is even across the contact area of the platen.
5.2 Data acquisition
Thickness measurements shall be obtained with a calibrated sensor capable of direct measurement of the distance between the compression platens. Examples include:
- — extensometer;
- — laser displacement measurement;
- — linear variable differential transformer (LVDT).
The accuracy of the displacement sensor shall be ±0,01 mm.
The thickness measurements obtained via direct sensing methods can be supplemented by compliancecorrected thickness measurements taken from the crosshead displacement of the UTM. Details of this method are provided in Annex BAnnex B..
Load measurements are to be taken from the load cell of the UTM. The load cell shall have a valid calibration certificate. The error for the indicated load shall not exceed ±1 % of applied full load.
5.3 Temperature conditions
The test shall be performed under isothermal conditions.
ISO/PRF 24819:2026(en)
5.4 Calculation of the fibre volume fraction
The thickness used in the test is equivalent to the displacement between platens. This can be related to the fibre volume fraction using Formula (1)Formula (1)::
𝐴𝐴 𝑛𝑛𝐴𝐴 ⋅𝑛𝑛 𝑤𝑤∙ w 𝑉𝑉𝑉𝑉 = 𝑓𝑓 f 𝜌𝜌∙𝑡𝑡 𝜌𝜌⋅𝑡𝑡 (1) where t is the thickness of the fabric; Aw is the areal weight of the fabric; n is the number of layers of fabric in the specimen; ρ is the density of a fibre the fabric; Vf is the fibre volume fraction.
Formula (1) (1) assumes that the reinforcement consists of one type of fibre. If more than one fibre material is used, or if additional materials are present in the reinforcement, such as polymeric powder binder or stitching yarns, this shall be considered by calculating separate volume fractions for each material component, from their respective areal densities and material densities, and then adding up the component volume fractions. In this case, one should use the term “solid volume fraction” (the sum of volume fractions of all components) to point out that the solid volume consists of more than one type of reinforcing fibres or other solids. The test can be based on either a set thickness or a set volume fraction. To test at a set volume fraction, the thickness used during testing shall be calculated from Formula (1) (1)..
...