IEC TS 62607-4-10:2026
(Main)Nanomanufacturing - Key control characteristics - Part 4-10: Nano-enabled energy storage - Electrochemical characteristics of carbon nanomaterial for the electrodes of electric double-layer capacitors: coin cell method
- Abstract
IEC TS 62607-4-10:2026, which is a Technical Specification, establishes standardized methods to determine the electrochemical key control characteristics, including:
• specific capacitance, voltage maintenance rate, endurance in cycling and temperature endurance of carbon nanomaterials by determining the standard coin-type EDLC.
The electrochemical key control characteristics are derived by calculating the recording curve at the specific charging and discharging process.
• The document is applicable for coin-type EDLC assembled from carbon nanomaterials, such as nanoporous activated carbon, carbon aerogel, carbon nanotube, carbon black, graphene, nano graphite sheet, vapor-grown carbon fibre and so on.
• Typical application areas of this method are research, manufacturer and downstream use to guide material processing and quality control.
- Status
- Published
- Publication Date
- 13-Jul-2026
- Technical Committee
- TC 113 - Nanotechnology for electrotechnical products and systems
- Drafting Committee
- WG 11 - Nano-enabled energy storage
- Current Stage
- PPUB - Publication issued - 60 Publication
- Start Date
- 14-Jul-2026
- Due Date
- 24-Jul-2026
- Completion Date
- 24-Jul-2026
Buy Documents
IEC TS 62607-4-10:2026 - Nanomanufacturing - Key control characteristics - Part 4-10: Nano-enabled energy storage - Electrochemical characteristics of carbon nanomaterial for the electrodes of electric double-layer capacitors: coin cell method
IEC TS 62607-4-10:2026 is a Technical Specification from the IEC for evaluating the electrochemical key control characteristics of carbon nanomaterials used in the electrodes of electric double-layer capacitors (EDLCs). It specifies coin-cell test methods for specific capacitance, voltage maintenance rate, endurance in cycling, and temperature endurance, so laboratories, manufacturers, and downstream users can compare materials in a consistent way. The methods are based on standard coin-type EDLCs assembled from the carbon nanomaterial under test.
What does IEC TS 62607-4-10:2026 specify?
IEC TS 62607-4-10:2026 specifies how to measure electrochemical performance of carbon nanomaterials in coin-type EDLCs. It covers the test setup, the charging and discharging sequences, the calculation approach, and the information that should be reported.
The document applies to coin-type EDLCs assembled from carbon nanomaterials such as nanoporous activated carbon, carbon aerogel, carbon nanotube, carbon black, graphene, nano graphite sheet, and vapor-grown carbon fibre. In practice, that means the method is aimed at materials used as active material or conductive material in EDLC electrodes.
The document is organized into:
- Clause 1 Scope
- Clause 2 Normative references
- Clause 3 Terms and definitions
- Clause 4 General
- Clause 5 Measurement
- Clause 6 Results to be reported
- Annex A Informative test report
- Annex B Informative case study for nanoporous activated carbon
| Annex | What it covers |
|---|---|
| A | Test report structure and reporting guidance |
| B | Worked case study for nanoporous activated carbon, including equipment, calculations, and example results |
What are the key requirements of IEC TS 62607-4-10:2026?
IEC TS 62607-4-10:2026 turns the material under test into standard coin-type EDLCs first, then uses those cells to measure the key electrochemical characteristics. The main value of the document is that it fixes the test sequence, the test conditions, and the way results are reduced to one reported value.
Sample preparation and test flow
Clause 4.1 requires the carbon nanomaterial to be assembled into standard coin-type EDLCs in accordance with IEC TS 62607-4-9. For a single carbon nanomaterial sample, at least 12 coin-type EDLCs are prepared. This matters because the test uses multiple cells, and the same cell is not reused across all methods.
Clause 4.2 says the cells are pre-conditioned before testing. It also says specific capacitance is measured first, then suitable cells are selected for the other tests. In practice, this keeps the reference state common across the later rate, retention, cycling, and temperature tests.
Test conditions and equipment
Clause 4.3 places the work under standard atmospheric conditions: 25 °C ± 2 °C, relative humidity 25 % to 75 %, and air pressure 86 kPa to 106 kPa. Clause 4.4 requires a potentiostat/galvanostat that can do constant current charging (CCC), constant voltage charging (CVC), and constant current discharging (CCD), while recording current and voltage over time.
Clause 4.4.2 also requires an environmental heating chamber for temperature endurance testing, with a maximum temperature of at least 90 °C and temperature control accuracy no worse than ± 2 °C. That makes the method suitable for comparing heat-aging behavior in a controlled way.
Specific capacitance
Clause 5.2 uses a CCC-CVC-CCD sequence. The cells are charged at 200 mA/g, held at the rated voltage for 1 800 s, then discharged to near zero voltage. The capacitance is calculated from the discharge segment between 0.8 and 0.4 of rated voltage, and the specific capacitance is then normalized to the active material mass.
For reporting, at least six coin-type EDLCs are used, and the final value is the arithmetic mean when the relative standard deviation of the replicate results is within the stated limit. In practice, this is the main baseline number for comparing carbon nanomaterials.
Rate capacitance
Clause 5.3 measures how well the material holds capacitance when the current is increased. It uses at least three coin-type EDLCs from the specific capacitance test and repeats the CCC-CVC-CCD method at 5C, 10C, 60C, and 100C.
The reported result is the retention of specific capacitance at each rate relative to the initial value. This matters because a material that looks good at low current may lose usable capacitance when the device is charged and discharged faster.
Voltage maintenance rate
Clause 5.4 measures self-discharge behavior. The cells are charged at 5C, held at constant voltage for 8 h, disconnected, and then left on open circuit while the terminal voltage is tracked for up to 72 h.
The voltage maintenance rate is the ratio of the remaining voltage to the rated voltage after the open-circuit period. In practice, this tells you how well the capacitor keeps its charge during storage or standby.
Endurance in cycling and temperature endurance
Clause 5.5 covers endurance in cycling. The cells are cycled with CCC and CCD, with short pauses, and the test continues until the capacitance falls to 80 % of the initial value, visible damage or electrolyte leakage is observed, or 100 000 cycles are reached.
Clause 5.6 covers temperature endurance. The cells are held in a high-temperature environment, then charged at constant voltage at that temperature, with checks at cumulative charging times up to 1 500 h. The test ends earlier if capacitance falls to 70 % of the initial value, damage or leakage appears, or the time limit is reached. In practice, this shows whether the material can survive heat stress while maintaining usable capacitance.
What terms does IEC TS 62607-4-10:2026 define?
- Electric double-layer capacitor (EDLC) - A device that stores energy electrostatically by charge separation in a double layer.
- Coin cell - A cylindrical cell whose height is less than its diameter, like a button cell.
- Active material - A material that stores energy through electric double-layer or pseudo-capacitance behavior.
- Activated carbon - Carbon treated to increase surface area and improve ion adsorption and desorption through a developed pore structure.
- Nanoporous activated carbon - Activated carbon that contains nanopores; its performance depends strongly on that pore structure.
- Upper category temperature - The highest ambient temperature, including internal heating, at which the capacitor is designed to operate continuously.
- Voltage maintenance rate - The ratio of the open-circuit terminal voltage to the charge voltage after a specified time.
- Endurance in cycling - The number of charge/discharge cycles until capacitance or internal resistance reaches a specified limit.
- Temperature endurance - The remaining capacitance or internal resistance after charging under a specified high temperature for a specified time.
Who uses IEC TS 62607-4-10:2026?
IEC TS 62607-4-10:2026 is used by research laboratories, material suppliers, capacitor manufacturers, and downstream users who need to compare carbon nanomaterials for EDLC electrodes. It is especially relevant to teams doing material processing, product qualification, and quality control.
For a quality manager or buyer, the document is useful when a supplier claims electrochemical performance for a carbon material and you need a repeatable way to check it. For an engineer, it gives a common test route for screening materials intended for coin-type EDLC prototypes or benchmarking.
Which standards are used with IEC TS 62607-4-10:2026?
- IEC TS 62565-5-1:2023 - Provides the blank detail specification for nanoporous activated carbon and is used for sample identification and reporting structure.
- IEC TS 62607-4-9 - Defines coin cell preparation for carbon nanomaterial EDLC electrodes and is the assembly basis for the tests in this document.
What does the IEC TS 62607-4-10:2026 document contain?
IEC TS 62607-4-10:2026 contains the full test workflow from sample assembly to reporting. Clause 4 describes preparation of the coin-type EDLCs, the test sequence, the required test conditions, and the equipment needed. Clause 5 gives the measurement procedures for specific capacitance, rate capacitance, voltage maintenance rate, endurance in cycling, and temperature endurance.
Clause 6 defines what has to be reported, including sample identification, assembly information, and each test result together with its test conditions. Annex A provides a report template, while Annex B gives a worked case study for nanoporous activated carbon with example equipment, voltage-time curves, calculations, and result tables. The document also includes figures that show the test arrangements and result interpretation for each method.
Buy Documents
IEC TS 62607-4-10:2026 - Nanomanufacturing - Key control characteristics - Part 4-10: Nano-enabled energy storage - Electrochemical characteristics of carbon nanomaterial for the electrodes of electric double-layer capacitors: coin cell method
Frequently Asked Questions
IEC TS 62607-4-10:2026 is a technical specification published by the International Electrotechnical Commission (IEC). Its full title is "Nanomanufacturing - Key control characteristics - Part 4-10: Nano-enabled energy storage - Electrochemical characteristics of carbon nanomaterial for the electrodes of electric double-layer capacitors: coin cell method". This standard covers: IEC TS 62607-4-10:2026, which is a Technical Specification, establishes standardized methods to determine the electrochemical key control characteristics, including: • specific capacitance, voltage maintenance rate, endurance in cycling and temperature endurance of carbon nanomaterials by determining the standard coin-type EDLC. The electrochemical key control characteristics are derived by calculating the recording curve at the specific charging and discharging process. • The document is applicable for coin-type EDLC assembled from carbon nanomaterials, such as nanoporous activated carbon, carbon aerogel, carbon nanotube, carbon black, graphene, nano graphite sheet, vapor-grown carbon fibre and so on. • Typical application areas of this method are research, manufacturer and downstream use to guide material processing and quality control.
IEC TS 62607-4-10:2026, which is a Technical Specification, establishes standardized methods to determine the electrochemical key control characteristics, including: • specific capacitance, voltage maintenance rate, endurance in cycling and temperature endurance of carbon nanomaterials by determining the standard coin-type EDLC. The electrochemical key control characteristics are derived by calculating the recording curve at the specific charging and discharging process. • The document is applicable for coin-type EDLC assembled from carbon nanomaterials, such as nanoporous activated carbon, carbon aerogel, carbon nanotube, carbon black, graphene, nano graphite sheet, vapor-grown carbon fibre and so on. • Typical application areas of this method are research, manufacturer and downstream use to guide material processing and quality control.
IEC TS 62607-4-10:2026 is classified under the following ICS (International Classification for Standards) categories: 07.120 - Nanotechnologies. The ICS classification helps identify the subject area and facilitates finding related standards.
IEC TS 62607-4-10:2026 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.
Standards Content (Sample)
Contents
- 1 Scope
- 2 Normative references
- 3 Terms and definitions
- 3.1 electric double-layer capacitor
- 3.2 coin cell
- 3.3 active material
- 3.4 activated carbon
- 3.5 nanoporous activated carbon
- 3.6 upper category temperature
- 3.7 applied voltage
- 3.8 rated voltage
- 3.9 charge current
- 3.10 discharge current
- 3.11 calculation start voltage
- 3.12 calculation end voltage
- 3.13 capacitance
- 3.14 constant current charging
- 3.15 constant voltage charging
- 3.16 constant current discharging
- 3.17 specific capacitance
- 3.18 voltage maintenance rate
- 3.19 endurance in cycling
- 3.20 temperature endurance
- 4 General
- 4.1 Preparation of the coin-type EDLCs of the tested carbon nanomaterial
- 4.2 Overview of the test
- 4.3 Test conditions
- 4.4 Description of measurement equipment / apparatus
- 5 Measurement
- 5.1 Pre-conditioning of the coin-type EDLC samples
- 5.2 Specific capacitance
- 1 R 2 R
- 5.3 Rate capacitance
- 5.4 Voltage maintenance rate
- 5.5 Endurance in cycling
- 5.6 Temperature endurance
- 6 Results to be reported
- 6.1 General
- 6.2 Sample identification
- 6.3 Assembly information of the coin-type EDLC
- 1 Slurry information
- 2 Current collector and separator Information Type, thickness, surface density and diameter
- 3 Electrode disc Information
- 4 Electrolyte Information Solvent, electrolyte and injection volume
- 5 Coin-type EDLC Information
- 6.4 Test results
- Annex A
- 1.1 Sample name
- 1.2 Function
- 1.3 Supplier
- 1.4 Trade name
- 1.5 Batch number
- 1.6 Typical batch quantity [ ] kg
- 1.7 Manufacturing date
- 1.8 Material safety data sheet (MSDS) available
- 1.9 Shelf life [ ] months
- Annex B
- 1.1 Sample name BC-10 nanoporous activated carbon
- 1.2 Function
- 1.3 Supplier SXICC
- 1.4 Trade name XXX
- 1.5 Batch number 20211008-DH
- 1.6 Typical batch quantity [ 20 ] kg
- 1.8 Material safety data sheet (MSDS) available
- 1.9 Shelf life [ 24 ] months
- Bibliography
INTRODUCTION Electrochemical capacitors are widely used in electric vehicles, high-speed trains, aviation, photovoltaics, wind power and electronics, due to their ultra-fast charge/discharge capability, long cycle life, wide working temperature range, high safety and reliability and low maintenance costs.
Electric double-layer capacitors (EDLCs) are a category of the electrochemical capacitors. The mechanism of energy storage for EDLCs relies on reversible ion adsorption at the interface between the active material and electrolyte. Therefore, materials with a large specific surface area - such as nanoporous carbon materials - are commonly employed as active materials in EDLCs. Additionally, to enhance electrode conductivity, high-conductivity materials (e.g. carbon black, graphene, and carbon nanotubes/CNTs) serve as conductive agents in EDLCs. Thus, carbon nanomaterials play an irreplaceable and critical role in EDLCs, directly determining their electrochemical performance.
The electrochemical performance of the carbon nanomaterial used in EDLC is evaluated using the assembled device, like coin-type EDLCs, three-electrode EDLC cells or cylindrical EDLC cells. Coin-cell-based characterization offers advantages including low cost, versatility, and high efficiency, making it widely used in both academic and industrial settings. This document introduces standard methods to determine the electrochemical key control characteristics of the carbon nanomaterial based on the coin-type EDLCs.
1 Scope
This part of IEC TS 62607 establishes standardized methods to determine the electrochemical key control characteristics, including:
- specific capacitance, voltage maintenance rate, endurance in cycling and temperature endurance of carbon nanomaterials by determining the standard coin-type EDLC. The electrochemical key control characteristics are derived by calculating the recording curve at the specific charging and discharging process.
- The document is applicable for coin-type EDLC assembled from carbon nanomaterials, such as nanoporous activated carbon, carbon aerogel, carbon nanotube, carbon black, graphene, nano graphite sheet, vapor-grown carbon fibre and so on.
- Typical application areas of this method are research, manufacturer and downstream use to guide material processing and quality control.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes requirements of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies.
IEC TS 62565-5-1:2023, Nanomanufacturing - Product specifications - Part 5-1: Nanoporous activated carbon - Blank detail specification: Electrochemical capacitor IEC TS 62607-4-9, Nanomanufacturing - Key control characteristics - Part 4-9: Nano-enabled energy storage - Electrochemical characteristics of carbon nanomaterial for the electrodes of electric double layer capacitors (EDLC): Coin cell preparation
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply. ISO and IEC maintain terminology databases for use in standardization at the following addresses:
- IEC Electropedia: available at https://www.electropedia.org/
- ISO Online browsing platform: available at https://www.iso.org/obp
3.1 electric double-layer capacitor
EDLC device for electrostatic storage of electrical energy achieved by separation of charge in a double layer [SOURCE: ISO 18300:2016, 3.8]
3.2 coin cell
cell with a cylindrical shape in which the overall height is less than the diameter e.g. in the shape of a button or a coin Note 1 to entry: In practice, the term coin is used exclusively for non-aqueous lithium cells. Note 2 to entry: Button cell is equivalent to coin cell.
[SOURCE: IEC 60050-482:2004, 482-02-40, modified - "button cell" has been moved to a note 2 to entry.]
3.3 active material
material that can be used to store energy by electrochemical double-layer or pseudo capacitance effect Note 1 to entry: Typically, nonreactive carbon materials are electric double-layer capacitance active material, including activated carbon, pure carbon nanotube and pure graphene. Note 2 to entry: Typically, carbon composites and carbons embedded with heteroatoms are pseudo capacitance active material..
[SOURCE: IEC TS 62565-5-2:2022, 3.3.1]
3.4 activated carbon
carbon, usually in the form of granules, treated to enhance its surface area and consequent ability to adsorbs/desorbs the ions through a highly developed pore structure Note 1 to entry: Activated charcoal is equivalent to activated carbon. [SOURCE: IEC TS 62565-5-1:2023, 3.2.5, modified - "activated charcoal" has been moved to a note 1 to entry.]
3.5 nanoporous activated carbon
activated carbon with nanopores Note 1 to entry: The performance of such activated carbon application mainly depends on its nanoporous structure. [SOURCE: IEC TS 62565-5-1:2023, 3.2.6]
3.6 upper category temperature
highest ambient temperature including internal heating in which a capacitor is designed to operate continuously [SOURCE: IEC 62391-1:2022, 3.40]
3.7 applied voltage
voltage (V) applied between the terminals of a capacitor [SOURCE: IEC 62576:2018, 3.2]
3.8 rated voltage
U R maximum DC voltage (V) that may be applied continuously for a certain time under the upper category temperature to a capacitor so that a capacitor can exhibit specified demand characteristics Note 1 to entry: This voltage is the setting voltage in capacitor design. [SOURCE: IEC 62576:2018, 3.20, modified – Note 2 has been deleted.]
3.9 charge current
I
current (A) required to charge a capacitor [SOURCE: IEC 62576:2018, 3.7]
3.10 discharge current
I d current (A) required to discharge a capacitor [SOURCE: IEC 62576:2018, 3.11]
3.11 calculation start voltage
voltage (V) at a selected start point for calculating the characteristics including capacitance under a state of voltage decrease during discharge [SOURCE: IEC 62576:2018, 3.4]
3.12 calculation end voltage
voltage (V) at a selected end point for calculating the characteristics including capacitance under a state of voltage decrease during discharge [SOURCE: IEC 62576:2018, 3.3]
3.13 capacitance
ability of a capacitor to store electrical charge Note 1 to entry: Unit: farad (F).
[SOURCE: IEC 62576:2018, 3.5, modified - information on units has been moved to Note 1 to entry.]
3.14 constant current charging
CCC charge during which the electric current is maintained at a constant value regardless of the voltage or temperature [SOURCE: IEC 60050-482:2004, 482-05-38]
3.15 constant voltage charging
CVC charge during which the voltage is maintained at a constant value regardless of charge current or temperature [SOURCE: IEC 60050-482:2004, 482-05-49]
3.16 constant current discharging
CCD discharge during which the electric current is maintained at a constant value regardless of the voltage or temperature
3.17 specific capacitance
capacitance of capacitor divided by the mass or volume of active material
Note 1 to entry: Unit: farad per gram (F/g) or farad per cubic centimetre (F/cm ) [SOURCE: IEC TS 62565-5-1:2023, 3.6.3]
3.18 voltage maintenance rate
ratio of voltage maintenance ratio of the voltage at the open-ended terminals to the charge voltage after a specified time period subsequent to the charging of a capacitor [SOURCE: IEC 62576:2018, 3.25]
3.19 endurance in cycling
number of charge and discharge cycles when the measured capacitance or internal resistance value reaches a specified degree of its initial value under a certain temperature and a certain rate of charge current [SOURCE: IEC TS 62565-5-1:2023, 3.6.6]
3.20 temperature endurance
ratio of the capacitance or internal resistance to its initial value after a specified charging time at constant voltage charge under a certain temperature [SOURCE: IEC TS 62565-5-1:2023, 3.6.7]
4 General
4.1 Preparation of the coin-type EDLCs of the tested carbon nanomaterial
Prior to measuring the electrochemical key control characteristics, the carbon nanomaterial under test shall be assembled into standard coin-type EDLCs in accordance with IEC TS 62607-4-9. For characterizing the key electrochemical characteristics of a single carbon nanomaterial sample, at least 12 coin-type EDLCs shall be prepared.
4.2 Overview of the test
4.2.1 Test sequence
Before the test, all the coin-type EDLCs shall be pre-conditioned. Notably, the known capacitance of each coin-type EDLC serves as foundational reference for tests including rate capacitance, voltage maintenance rate, endurance in cycling and temperature endurance. To ensure the reliability of test results, replicate EDLCs within a single test, for instance, the three parallel coin-type EDLCs used in the rate capacitance test shall be in identical states. Furthermore, each coin-type EDLC is dedicated to only one of the four aforementioned tests (rate capacitance, voltage maintenance rate, endurance in cycling and temperature endurance) and shall not be reused across different test types.
Therefore, it is suggested to test the specific capacitance of all assembled coin-type EDLCs first, then select at least three suitable coin-type EDLCs for the other tests. The test sequence of electrochemical key characteristics and the corresponding number of the sample coin-type EDLCs required for each testing are shown in Figure 1, where the references to the specific clauses are also given.
Figure 1 – Overview of the test
4.2.2 Test efficiency
The times for testing the specific capacitance and rate capacitance, voltage maintenance rate, endurance in cycling and temperature endurance are about 1 h, 2 h, 81 h, 73 h, 2 522 h and 1 644 h, respectively.
The rate capacitance, voltage maintenance rate, endurance in cycling and temperature endurance test are optional test and shall be agreed between manufacturer and user.
4.3 Test conditions
Unless otherwise specified, all procedures shall be operated under standard atmospheric conditions as following:
- Temperature: 25 °C ± 2 °C.
- Relative humidity: 25 % to 75 %.
- Air pressure: 86 kPa to 106 kPa.
4.4 Description of measurement equipment / apparatus
4.4.1 Potentiostat/galvanostat equipment
The potentiostat/galvanostat equipment shall be capable of constant current charging (CCC), constant voltage charging (CVC), constant current discharging (CCD), and can continuously measure and record the current and the voltage between the capacitor terminals in time-series.
4.4.2 Environmental heating chamber
The chamber shall be allowed to adjust the temperature. The maximum temperature of the chamber shall be no smaller than 90 °C. The temperature control accuracy shall be no lower than ± 2 °C.
5 Measurement
5.1 Pre-conditioning of the coin-type EDLC samples
Connect the prepared coin-type capacitors with the potentiostat/galvanostat equipment. Charge the coin-type EDLCs at a constant current density of 200 mA/g to U and maintain this R voltage for 30 min. Next, fully discharge the coin-type EDLCs to (0 to 0,1) V at the same current density, followed by resting them in the test environment outlined in 4.3 for at least 12 h. Keep all coin-type EDLCs connected with the potentiostat/galvanostat equipment for other tests at the test condition stated in 4.3 unless otherwise specified.
5.2 Specific capacitance
5.2.1 Charging and discharging process (CCC-CVC-CCD)
a) CCC: Charge the coin-type EDLC at a constant current of I . The I , expressed in cc cc milliamperes (mA), can be calculated as follows:
Im200× (1)
where 200 is the charging current density, expressed in milliamperes per gram (mA/g); m is the mass of the carbon nanomaterials used as active material in a single electrode disc, expressed in grams (g). If the masses of the two electrode discs differ, the smaller mass shall be used.
b) CVC: When the output voltage of the coin-type EDLC reaches the specified value U , R continue charging the coin-type EDLC sample at a constant voltage of U for a constant- R voltage charging duration (T ) of 1 800 s. Typically, U is 2,7 V; if not, it shall be specified CV R in the test conditions.
c) CCD: Discharge the coin-type EDLC to a voltage range of (0 to 0,1) V at a constant current of I , where I is equal to the I .
dc dc cc d) The time shall be measured from the start of discharge to the points where the voltage across the capacitor terminals reaches U = 0,8 × U and U = 0,4 × U , respectively (see
1 R 2 R
Figure 2).
e) For specific capacitance testing, at least six coin-type EDLCs shall be used for each type of carbon nanomaterial.
Key U rated voltage (V); R U calculation start voltage (V);
U calculation end voltage (V);
∆U voltage drop (V);
T constant voltage charging duration (s).
CV Figure 2 – Voltage–time profile of the coin-type EDLC during the CCC-CVC-CCD process
5.2.2 Data analysis
5.2.2.1 Capacitance of a coin-type EDLC
The capacitance C of the coin-type EDLC sample shall be calculated as follows:
I ×−(tt) dc 2 1 C= (2) UU−
...