ASTM D1876-08
(Test Method)Standard Test Method for Peel Resistance of Adhesives (T-Peel Test)
Standard Test Method for Peel Resistance of Adhesives (T-Peel Test)
ABSTRACT
This test method is primarily intended for determining the relative peel resistance of adhesive bonds between flexible adherends by means of a T-type specimen using a tension testing machine. The bent, unbonded ends of the test specimen shall be clamped in the test grips of the tension testing machine and a load of a constant head speed shall be applied. An autographic recording of the load versus the head movement or load versus distance peeled shall be made. The peel resistance over a specified length of the bond line after the initial peak shall be determined.
SCOPE
1.1 This test method is primarily intended for determining the relative peel resistance of adhesive bonds between flexible adherends by means of a T-type specimen.
1.2 The values stated in SI units are to be regarded as the standard. The values given in parentheses are provided for information purposes only.
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.
General Information
Relations
Buy Standard
Standards Content (Sample)
NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D1876 − 08
StandardTest Method for
1
Peel Resistance of Adhesives (T-Peel Test)
This standard is issued under the fixed designation D1876; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the Department of Defense.
INTRODUCTION
The accuracy of the results of strength tests of adhesive bonds will depend on the conditions under
which the bonding process is carried out. Unless otherwise agreed upon by the manufacturer and the
purchaser, the bonding conditions shall be prescribed by the manufacturer of the adhesive. In order to
ensure that complete information is available to the individual conducting the tests, the manufacturer
of the adhesive shall furnish numerical values and other specific information for each of the following
variables:
(1) Procedure for preparation of the surfaces prior to application of the adhesive, the cleaning and
drying of metal surfaces, and special surface treatments such as sanding, which are not specifically
limited by the pertinent test method.
(2) Complete mixing directions for the adhesive.
(3) Conditions for application of the adhesive, including the rate of spread or thickness of film,
number of coats to be applied, whether to be applied to one or both surfaces, and the conditions of
drying where more than one coat is required.
(4) Assembly conditions before application of pressure, including the room temperature, length of
time, and whether open or closed assembly is to be used.
(5) Curing conditions, including the amount of pressure to be applied, the length of time under
pressure, and the temperature of the assembly when under pressure. It should be stated whether this
temperature is that of the glue line, or of the atmosphere at which the assembly is to be maintained.
(6) Conditioning procedure before testing, unless a standard procedure is specified, including the
length of time, temperature, and relative humidity.
Arangemaybeprescribedforanyvariablebythemanufactureroftheadhesive,ifitcanbeassumed
by the test operator that any arbitrarily chosen value within such a range or any combination of such
values for several variables will be acceptable to both the manufacturer and the purchaser of the
adhesive.
1. Scope responsibility of the user of this standard to establish appro-
priate safety and health practices and determine the applica-
1.1 This test method is primarily intended for determining
bility of regulatory limitations prior to use.
the relative peel resistance of adhesive bonds between flexible
adherends by means of a T-type specimen.
2. Referenced Documents
2
1.2 The values stated in SI units are to be regarded as the
2.1 ASTM Standards:
standard. The values given in parentheses are provided for
B209 Specification for Aluminum and Aluminum-Alloy
information purposes only.
Sheet and Plate
D907 Terminology of Adhesives
1.3 This standard does not purport to address all of the
safety concerns, if any, associated with its use. It is the
3. Terminology
3.1 Definitions:
1
This test method is under the jurisdiction of ASTM Committee D14 on
2
Adhesives and is the direct responsibility of D14.80 on Metal Bonding Adhesives. For referenced ASTM standards, visit the ASTM website, www.astm.org, or
Current edition approved Oct. 1, 2008. Published October 2008. Originally contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM
approved in 1961. Last previous edition approved in 2001 as D1876 – 01. DOI: Standards volume information, refer to the standard’s Document Summary page on
10.1520/D1876-08. the ASTM website.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United States
1
---------------------- Page: 1 ----------------------
D1876 − 08
3.1.1 Many terms in this test method are defined in Termi- 4.2 Conditioning Room or Desiccators—The conditioning
nology D907. room or desiccators (Note 2) shall be capable of maintaining a
3.1.2 peel strength, n—the average load per unit width of relative humidity of 50 6 2 % at 23 6 1°C (73.4 6 1.8°F).
bondline required to separate progressively a flexible member
NOTE 2—A saturated solution of calcium nitrate will give approxi-
from a rigid member or another flexible member.
mately 51 % relative humidity at the testing temperature.
3.1.2.1 Discussion—Flexible has different meanings in dif-
ferent peel tests, such as “T,” 180-degree, floating-roller, or
5. Test Specimen
climbing-drum. The angle between the members varies with
5.1 Laminated test panels (see Fig. 1) consist of two flexible
the type of pe
...
This document is not an ASTM standard and is intended only to provide the user of an ASTM standard an indication of what changes have been made to the previous version. Because
it may not be technically possible to adequately depict all changes accurately, ASTM recommends that users consult prior editions as appropriate. In all cases only the current version
of the standard as published by ASTM is to be considered the official document.
Designation:D1876–01 Designation: D 1876 – 08
Standard Test Method for
1
Peel Resistance of Adhesives (T-Peel Test)
This standard is issued under the fixed designation D 1876; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
This standard has been approved for use by agencies of the Department of Defense.
INTRODUCTION
The accuracy of the results of strength tests of adhesive bonds will depend on the conditions under
which the bonding process is carried out. Unless otherwise agreed upon by the manufacturer and the
purchaser, the bonding conditions shall be prescribed by the manufacturer of the adhesive. In order to
ensure that complete information is available to the individual conducting the tests, the manufacturer
of the adhesive shall furnish numerical values and other specific information for each of the following
variables:
(1) Procedure for preparation of the surfaces prior to application of the adhesive, the cleaning and
drying of metal surfaces, and special surface treatments such as sanding, which are not specifically
limited by the pertinent test method.
(2) Complete mixing directions for the adhesive.
(3) Conditions for application of the adhesive, including the rate of spread or thickness of film,
number of coats to be applied, whether to be applied to one or both surfaces, and the conditions of
drying where more than one coat is required.
(4) Assembly conditions before application of pressure, including the room temperature, length of
time, and whether open or closed assembly is to be used.
( 5) Curing conditions, including the amount of pressure to be applied, the length of time under
pressure, and the temperature of the assembly when under pressure. It should be stated whether this
temperature is that of the glue line, or of the atmosphere at which the assembly is to be maintained.
(6) Conditioning procedure before testing, unless a standard procedure is specified, including the
length of time, temperature, and relative humidity.
Arangemaybeprescribedforanyvariablebythemanufactureroftheadhesive,ifitcanbeassumed
by the test operator that any arbitrarily chosen value within such a range or any combination of such
values for several variables will be acceptable to both the manufacturer and the purchaser of the
adhesive.
1. Scope
1.1 This test method is primarily intended for determining the relative peel resistance of adhesive bonds between flexible
adherends by means of a T-type specimen.
1.2 ThevaluesstatedinSIunitsaretoberegardedasthestandard.Thevaluesgiveninparenthesesareprovidedforinformation
purposes only.
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility
of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory
limitations prior to use.
2. Referenced Documents
2
2.1 ASTM Standards:
B 209 Specification for Aluminum and Aluminum-Alloy Sheet and Plate
1
This test method is under the jurisdiction of ASTM Committee D14 on Adhesives and is the direct responsibility of D14.80 on Metal Bonding Adhesives.
{1
Current edition approved Oct. 10, 2001. Published December 2001. Originally published as D1876–61 T. Last previous edition D1876–00 .
Current edition approved Oct. 1, 2008. Published October 2008. Originally approved in 1961. Last previous edition approved in 2001 as D 1876 – 01.
2
For referencedASTM standards, visit theASTM website, www.astm.org, or contactASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards
, Vol 02.02.volume information, refer to the standard’s Document Summary page on the ASTM website.
Copyright © ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.
1
---------------------- Page: 1 ----------------------
D1876–08
D 907 Terminology of Adhesives E4Practices for Force Verification of Testing Machines
3. Terminology
3.1 Definitions—Many terms in this test method are defined in Terminology D 907.
3.1.1 peel strength, n—the average load per unit width of bondline required to separate progressively a flexible member from
a rigid member or another flexible member.
3.1.1.1 Discussion—Flexible has different meanings in different peel tests, such as “T”,“T,” 180-degree, floating-roller,
...
Questions, Comments and Discussion